Method for regulating and controlling mechanical properties of dental titanium alloy based on nitrogen element

The powder metallurgy method is used to heat nitriding and high-energy ball milling of Ti powder, combined with the vacuum hot pressing sintering process, to solve the problem of uneven distribution of nitrogen elements in titanium alloys, significantly improve the strength and toughness of titanium alloys, simplify the process flow and Improved production efficiency.

CN118745536APending Publication Date: 2024-10-08CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410799753.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing technology makes it difficult to uniformly control the nitrogen content when preparing titanium alloys for dental use, resulting in loss of material strength and toughness, and traditional smelting methods are prone to segregation and inclusion problems.

Method used

The powder metallurgy method is used to heat nitriding and high-energy ball milling of the Ti powder, combined with the vacuum hot-pressing sintering process, to accurately control the distribution of nitrogen elements and form a uniform Ti-Zr alloy.

Benefits of technology

It achieves precise control of the nitrogen element in titanium alloys, significantly improves the strength and toughness of the material, avoids segregation and inclusion problems in the smelting method, simplifies the process, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745536A_ABST
    Figure CN118745536A_ABST
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the mechanical property of a dental titanium alloy based on a nitrogen element, and belongs to the technical field of metal materials. The method comprises the following steps that Ti powder is heated and nitrided, and nitrided Ti powder is obtained; the nitrided Ti powder is subjected to high-energy ball milling, and nitrided fine Ti powder is obtained; mixing the nitrided fine Ti powder with Zr powder to obtain mixed powder; the mixed powder is subjected to vacuum hot pressing sintering, and a titanium alloy sintered blank is obtained; and the titanium alloy sintered blank is subjected to deformation machining, and the titanium alloy material is obtained. According to the method, a powder metallurgy method is adopted, the raw material Ti powder is subjected to heating nitriding and crushing treatment, homogenization of nitrogen elements in the titanium alloy and accurate control over the nitrogen content can be achieved, and the high-strength and high-toughness titanium alloy material for the dental implant is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of metal materials, and in particular to a method for regulating the mechanical properties of a titanium alloy for dentistry based on nitrogen. Background Art

[0002] At present, titanium and titanium alloys have been widely used in biomedicine due to their high specific strength, high corrosion resistance and good biocompatibility, and are the basic materials for preparing oral implants. Early implants were mainly prepared using pure titanium as raw material, but their wear resistance and fatigue performance were relatively low. After being implanted in the human body, the surface was prone to wear, which then induced inflammation and mechanical damage, resulting in a short service life of the implant. Later, due to the good comprehensive properties of Ti6Al4V alloy, it was also widely used in clinical practice. However, in long-term clinical trials, it was found that Al and V elements were cytotoxic and easily caused oral inflammation, making them unsuitable for long-term use as dental implants. In recent years, Straumann, a well-known international dental company, has proposed using high-strength and toughness Ti-15Zr alloy as raw material to prepare dental implants, which have both high mechanical properties and excellent biocompatibility. However, the control of nitrogen content in titanium alloys is very important and is the main factor affecting the strength and toughness of materials. How to uniformly dissolve a relatively high concentration of nitrogen (0.3-0.6 wt.%) in a titanium alloy without causing nitride aggregation and precipitation is the key to preparing high-performance titanium alloys.

[0003] At present, the nitrogen control methods of metal materials mainly include the introduction of nitrogen-rich atmosphere or the addition of metal nitrides for mixed smelting during alloy smelting. For example, in the titanium alloy smelting process, by adding titanium or other metal nitrides as nitrogen sources and mixing with alloy raw materials for smelting, a nitrogen-containing titanium alloy with a relatively uniform composition can be obtained. Similarly, in the preparation process of nitrogen-rich high-entropy alloys, nitrogen is introduced as a nitrogen source and added to a suspension furnace for smelting, and finally a high-strength, high-toughness, high-entropy alloy with a nitrogen content of 0.5 to 1.5 at.% can be obtained. However, the above-mentioned nitrogen control method is difficult to apply to dental Ti-15Zr alloys, because the Zr element has a high affinity with nitrogen, and it is easy to react to form zirconium nitride during the smelting process. This substance will float to the surface of the ingot during the solidification process, resulting in a low nitrogen content inside the alloy ingot, and brittle nitride inclusions are formed on the surface of the alloy, which seriously damages the strength and toughness of the material. The powder metallurgy method has unique advantages in nitrogen content control due to its flexible composition control and does not involve liquid phase solidification. It is expected to solve the problem of precise control of nitrogen content in high-performance dental titanium alloys. Summary of the invention

[0004] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen to solve the above problems existing in the prior art. The present invention adopts a powder metallurgy method to heat nitriding and high-energy ball milling (crushing) the raw material Ti powder, which can achieve the homogenization and content control of the nitrogen element in the titanium alloy.

[0005] The second object of the present invention is to provide a titanium alloy prepared by a method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen.

[0006] The third object of the present invention is to provide the use of the above titanium alloy in the preparation of oral implants.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] The present invention discloses a method for regulating the mechanical properties of titanium alloy for dentistry based on nitrogen element, comprising the following steps: heating Ti powder to nitridize to obtain nitrided Ti powder; high-energy ball milling the nitrided Ti powder to obtain nitrided fine Ti powder; mixing the nitrided fine Ti powder with Zr powder to obtain mixed powder; sintering the mixed powder to obtain a titanium alloy sintered blank; and deforming the titanium alloy sintered blank to obtain a titanium alloy.

[0009] Furthermore, the titanium alloy is a titanium alloy plate or rod.

[0010] Furthermore, the particle size of the Ti powder is less than 45 μm, the nitrogen content is less than 0.1 wt.%, and the purity is ≥ 99%.

[0011] More preferably, the particle size of the Ti powder is 20-40 μm, and the nitrogen content is less than 0.05 wt.%.

[0012] Furthermore, the Ti powder is flaky Ti powder (ie, the shape of the Ti powder is flaky) and / or irregular Ti powder (ie, the shape of the Ti powder is irregular).

[0013] Further preferably, the Ti powder is flaky Ti powder. The inventors found that the surface of flaky Ti powder can be nitrided more evenly during the nitriding process, and the effect of irregular Ti powder is second, but both flaky Ti powder and irregular Ti powder are better than spherical Ti powder.

[0014] Furthermore, the heating nitriding temperature is 300-600° C., the time is 1-6 hours, and the nitrogen concentration is 60-90 vol.%.

[0015] In the present invention, the selection of heating nitriding parameters is a key step in controlling the nitrogen content in Ti powder after nitriding. The nitriding rate of Ti powder is mainly affected by the nitriding temperature, nitrogen concentration and nitriding time. As the nitriding temperature increases, the collision frequency between Ti powder and nitrogen molecules increases sharply, promoting the nitriding reaction. At the same time, increasing the nitrogen concentration and extending the nitriding time can increase the contact area between Ti powder and nitrogen and the diffusion depth of nitrogen atoms in Ti powder.

[0016] In addition, the inventors found that when the nitriding temperature is low, the nitriding concentration is too low or the nitriding time is too short, the nitrogen distribution in the core of the Ti powder is uneven and the content is low; when the nitriding temperature is too high, the nitriding rate of the Ti powder is extremely fast, and it is difficult to control the nitrogen content in the Ti powder even at a low nitriding concentration and a short nitriding time. Therefore, only under the preferred nitriding temperature, nitrogen concentration and nitriding time can the nitrogen content in the Ti powder be strictly controlled, and Ti powder with different nitrogen contents and uniform nitriding can be efficiently obtained.

[0017] Furthermore, the heating nitriding temperature is 300-350°C, the time is 1-3h, and the nitrogen concentration is 80-90vol.%;

[0018] or

[0019] The heating nitriding temperature is 350-400°C, the time is 3-6 hours, and the nitrogen concentration is 70-80 vol.%; or

[0020] The heating nitriding temperature is 400-450°C, the time is 1-3h, and the nitrogen concentration is 80-90vol.%; or

[0021] The heating nitriding temperature is 450-500°C, the time is 3-4 hours, and the nitrogen concentration is 70-80 vol.%; or

[0022] The heating nitriding temperature is 500-550°C, the time is 1-3h, and the nitrogen concentration is 70-80vol.%; or

[0023] The heating nitriding process is performed at a temperature of 550-600° C., for a time of 1-2 hours, and a nitrogen concentration of 60-70 vol.%.

[0024] The present invention adopts the above-mentioned preferred scheme, adopts a higher nitrogen concentration and different nitriding times in the low-temperature section (300-400°C) with a slower nitriding rate, so as to obtain Ti powder with a low nitrogen content and uniform nitrogen distribution; adopts a higher nitrogen concentration and a moderate nitriding time in the medium-temperature section (400-500°C) with a moderate nitriding rate, so as to obtain Ti powder with a medium nitrogen content and uniform nitrogen distribution; adopts a lower nitrogen concentration and a shorter nitriding time in the high-temperature section (500-600°C) with a higher nitriding rate, so as to obtain Ti powder with a high nitrogen content and uniform nitrogen distribution.

[0025] In the above preferred solution, the heating nitriding parameters and the nitrogen content in the nitrided Ti powder obtained after heating nitriding under the parameters are shown in Table 1:

[0026] Table 1

[0027] Nitriding temperature / ℃ Nitrogen concentration / vol.% Nitriding time / h Nitrogen content in Ti powder after nitriding / wt.% 300~350 80~90 1~3 0.18~0.32 350~400 70~80 3~6 0.30~0.45 400~450 80~90 1~3 0.42~0.53 450~500 70~80 3~4 0.51~0.59 500~550 70~80 1~3 0.57~0.62 550~600 60~70 1~2 0.60~0.68

[0028] Furthermore, the heating nitriding is carried out in a pot mill; the rotation speed of the pot mill is 10-20r / min.

[0029] Furthermore, the pot mill is a constant temperature atmosphere pot mill.

[0030] In the present invention, the nitrogen concentration during heat nitriding is the nitrogen concentration in the pot mill.

[0031] Furthermore, the rotation speed of the high-energy ball mill is 300-500 r / min, the time is 1-5 h, and the ball-to-material ratio is 5:1-7:1; and the particle size of the nitrided fine Ti powder is ≤20 μm.

[0032] Furthermore, the high-energy ball milling is carried out under an Ar gas protective atmosphere.

[0033] In the present invention, a dense nitride film is formed on the surface of the Ti powder after heating and nitriding. In the subsequent vacuum hot pressing sintering process, the presence of the nitride film will hinder the mutual diffusion and self-diffusion between Ti and Zr atoms, and the mixed powder body is difficult to densify and alloy. Therefore, the inventor uses high-energy ball milling to crush and mix the nitrided Ti powder evenly to improve the density and alloying degree of the sintered body.

[0034] In the actual operation process, the nitrided Ti powder needs to be taken out in a glove box filled with Ar gas and loaded into a ball mill to prevent the nitrided Ti powder from being nitrided again during the process of taking out and loading. Under the preferred high-energy ball milling process, the nitrided Ti powder is crushed and mixed evenly, which is conducive to improving the uniformity of the distribution of nitrogen in the sample.

[0035] Furthermore, the Zr powder has a particle size of <100 μm, a nitrogen content of <0.1 wt.%, and a purity of ≥99%.

[0036] Further preferably, the Zr powder has a particle size of 30-80 μm and a nitrogen content of <0.05 wt.%.

[0037] Furthermore, the mixing mass ratio of the nitriding fine Ti powder to the Zr powder is 80-95:5-20; and the mixing time is 4-10 hours.

[0038] Further preferably, the mixing mass ratio of the nitriding fine Ti powder to the Zr powder is 80-88:12-20.

[0039] In the actual operation process, nitriding fine Ti powder and Zr powder in a certain ratio are placed in the transition chamber of the glove box, and then put into the mixing tank, filled with Ar gas and the powder is packaged. Ar gas is used for protection throughout the process.

[0040] Furthermore, the mixing is carried out on a three-dimensional mixer.

[0041] More preferably, the mixing time is 6 to 8 hours.

[0042] Furthermore, the sintering is vacuum hot pressing sintering, the temperature of the vacuum hot pressing sintering is 1000-1500°C, the heating rate is 5-15°C / min, the pressure is 10-50MPa, the holding time is 0.5-4h, and the vacuum degree is <10 -3 Pa.

[0043] Further preferably, the vacuum hot pressing sintering temperature is 1200-1350°C, the heating rate is 10°C / min, the pressure is 20-40MPa, the holding time is 1-3h, and the vacuum degree is 5×10 -4 Pa.

[0044] Under the preferred vacuum hot pressing sintering process, the nitrided Ti powder and Zr powder exchange and diffuse elements through the solid phase sintering pathway, and the nitrogen element diffuses and distributes evenly in the Ti matrix, avoiding the occurrence of local enrichment of the nitrogen element.

[0045] Furthermore, the deformation process is selected from rolling, extrusion or forging, the deformation process temperature is 800-1100° C., and the deformation amount is 50-90%.

[0046] Further preferably, the deformation amount of the deformation processing is 80-90%, which can eliminate residual pores and defects and improve the density of the material.

[0047] The present invention also provides a titanium alloy prepared according to the above method for regulating the mechanical properties of titanium alloy for dentistry based on nitrogen element.

[0048] The present invention also provides application of the titanium alloy in preparing oral implants.

[0049] The present invention discloses the following technical effects:

[0050] (1) The present invention provides a method for regulating the mechanical properties of titanium alloy for dentistry based on nitrogen. Starting from the raw material Ti powder, the Ti powder is subjected to heating nitriding treatment to accurately control the nitrogen content in the Ti powder. The nitrided Ti powder is then crushed and evenly mixed by high-energy ball milling. The crushed nitrided Ti powder is mixed with Zr powder and then diffused with each other during vacuum hot pressing sintering to form a Ti-Zr alloy with uniform nitrogen distribution. Compared with the traditional nitrogen control method of adding metal nitrides for smelting, the nitrogen content control method of the present invention can achieve precise control of the nitrogen content in the Ti-Zr alloy (0.30-0.60wt.%), and the nitrogen element is evenly distributed in the alloy, which has a significant effect on improving the strength of the Ti-Zr alloy, and can keep the material plasticity from being significantly reduced, so as to obtain a titanium alloy material for oral implants with high strength and toughness.

[0051] (2) The process of the present invention is simple and time-saving, and can avoid the problems of segregation and inclusions that occur during the smelting preparation process. The equipment is simple and can efficiently produce Ti-Zr alloys with different nitrogen contents. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0053] Figure 1 It is a process flow chart of the present invention.

[0054] Figure 2 This is an axial SEM photograph of the powder metallurgy Ti-Zr alloy rod prepared in Example 1 of the present invention;

[0055] Figure 3 This is a nitrogen element distribution diagram of the powder metallurgy Ti-Zr alloy rod prepared in Example 1 of the present invention;

[0056] Figure 4 This is an axial SEM photograph of the powder metallurgy Ti-Zr alloy rod prepared in Comparative Example 1 of the present invention;

[0057] Figure 5 This is the nitrogen element distribution diagram of the powder metallurgy Ti-Zr alloy rod prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0058] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0059] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0060] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0061] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0062] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0063] The process flow of the following embodiments is as follows Figure 1 shown.

[0064] Example 1

[0065] A method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen is carried out in the following steps:

[0066] (1) Ti powder with a particle size of less than 45 μm (nitrogen content of 0.03 wt.%, purity of 99.2 wt.%) was used as a raw material and loaded into a constant temperature atmosphere jar mill for heating and nitriding. The nitriding temperature was 400°C, the nitrogen concentration was 70 vol.%, the speed of the constant temperature atmosphere jar mill was 15 r / min, and the nitriding time was 3 h to obtain nitrided Ti powder.

[0067] (2) The nitriding Ti powder is placed in a ball mill in a glove box, and the ball mill is tightened and placed in a planetary high-energy ball mill for high-energy ball milling. The ball mill speed is 400 r / min, the ball milling time is 2 h, and the ball-to-material ratio is 5:1 to obtain crushed nitriding fine Ti powder. The powder collection and powder loading in this process are carried out in the glove box, and Ar gas protection is used throughout the process.

[0068] (3) Weigh nitriding fine Ti powder and Zr powder (particle size <45 μm, nitrogen content of 0.02 wt.%, purity of 99.4 wt.%) in a mass ratio of nitriding fine Ti powder: Zr powder = 85:15, place the two metal powders in a transition chamber of a glove box under Ar gas environment, and put the two metal powders into a mixing tank in the transition chamber, fill the mixing tank with Ar gas and seal the powders, and then put the mixing tank into a three-dimensional mixer for uniform mixing for 6 hours to obtain a mixed powder.

[0069] (4) The mixed powder was loaded into a hot-pressed graphite mold and then placed in a vacuum hot-pressed sintering furnace. During the sintering process, the temperature was directly heated from room temperature to 1200°C at a heating rate of 10°C / min, the pressure was maintained at 30 MPa, the holding time was 2 h, and the vacuum degree was 5×10 -4 Pa, and a dense titanium alloy sintered billet is obtained.

[0070] (5) The titanium alloy sintered billet is hot forged at 800°C with a deformation amount of 90% to obtain a Ti-Zr alloy rod.

[0071] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.41wt.%, and the particle size of the nitrided fine Ti powder was 5-15μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and its SEM photo is as follows: Figure 2 As shown in FIG. 1 , it is found that the Zr element is completely dissolved in the Ti matrix; the distribution of nitrogen in the Ti-Zr alloy rod obtained by energy spectrum analysis step (5) is as follows: Figure 3 As shown, it is found that the nitrogen element is evenly distributed, and the nitrogen content obtained by test is 0.43wt.%; finally, according to "GBT 228.1-2010 Tensile test of metallic materials Part 1: Room temperature test method", the Ti-Zr alloy bar obtained in step (5) is subjected to a tensile test, and the tensile strength of the Ti-Zr alloy is measured to be 966MPa, the yield strength is 907MPa, the elongation is 21%, and the elastic modulus is 107GPa.

[0072] Example 2

[0073] A method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen is carried out in the following steps:

[0074] (1) Ti powder in the form of flakes with a particle size of 20 to 40 μm (nitrogen content of 0.05 wt.%, purity of 99.4 wt.%) was used as a raw material and loaded into a constant temperature atmosphere jar mill for heating and nitriding. The nitriding temperature was 350°C, the nitrogen concentration was 80 vol.%, the speed of the constant temperature atmosphere jar mill was 12 r / min, and the nitriding time was 2 h to obtain nitrided Ti powder.

[0075] (2) The nitriding Ti powder was placed in a ball mill in a glove box, and the ball mill was tightened and placed in a planetary high-energy ball mill for high-energy ball milling. The ball mill speed was 300 r / min, the ball milling time was 3 h, and the ball-to-material ratio was 7:1 to obtain crushed nitriding fine Ti powder. The powder collection and powder loading in this process were carried out in a glove box, and Ar gas protection was used throughout the process.

[0076] (3) Weigh nitriding fine Ti powder and Zr powder (particle size <45 μm, nitrogen content of 0.02 wt.%, purity of 99.1 wt.%) in a mass ratio of nitriding Ti powder: Zr powder = 85:15, place the two metal powders in a transition chamber of a glove box under Ar gas environment, and put the two metal powders into a mixing tank in the transition chamber, fill the mixing tank with Ar gas and seal the powder, and then put the mixing tank into a three-dimensional mixer for uniform mixing for 8 hours to obtain a mixed powder.

[0077] (4) The mixed powder was loaded into a hot-pressed graphite mold and then placed in a vacuum hot-pressed sintering furnace. During the sintering process, the temperature was directly heated from room temperature to 1000°C at a heating rate of 15°C / min, the pressure was maintained at 40 MPa, the pressure holding time was 3 h, and the vacuum degree was 5×10 -4 Pa, and a dense titanium alloy sintered billet is obtained.

[0078] (5) The titanium alloy sintered billet is hot extruded at 950° C. with a deformation amount of 85% to obtain a Ti—Zr alloy rod.

[0079] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.26wt.%, and the particle size of the nitrided fine Ti powder was 5-18μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix; the nitrogen element distribution in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen element was evenly distributed and the content was 0.29wt.%; finally, according to "GBT 228.1-2010 Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 830MPa, the yield strength was 756MPa, the elongation was 25%, and the elastic modulus was 104GPa.

[0080] Example 3

[0081] A method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen is carried out in the following steps:

[0082] (1) Irregular Ti powder with a particle size of less than 45 μm (nitrogen content of 0.02 wt.%, purity of 99.3 wt.%) was used as a raw material and loaded into a constant temperature atmosphere jar mill for heating nitriding. The nitriding temperature was 500°C, the nitrogen concentration was 80 vol.%, the speed of the constant temperature atmosphere jar mill was 10 r / min, and the nitriding time was 2 h to obtain nitrided Ti powder.

[0083] (2) The nitriding Ti powder is placed in a ball mill in a glove box, and the ball mill is tightened and placed in a planetary high-energy ball mill for high-energy ball milling. The ball mill speed is 400 r / min, the ball milling time is 3 h, and the ball-to-material ratio is 6:1 to obtain crushed nitriding fine Ti powder. The powder collection and powder loading in this process are carried out in the glove box, and Ar gas protection is used throughout the process.

[0084] (3) Weigh nitriding fine Ti powder and Zr powder (particle size <45 μm, nitrogen content of 0.02 wt.%, purity of 99.2 wt.%) in a mass ratio of nitriding fine Ti powder: Zr powder = 83:17, place the two metal powders in a transition chamber of a glove box under Ar gas environment, and put the two metal powders into a mixing tank in the transition chamber, fill the mixing tank with Ar gas and seal the powders, and then put the mixing tank into a three-dimensional mixer for uniform mixing for 10 hours to obtain a mixed powder.

[0085] (4) The mixed powder was loaded into a hot-pressed graphite mold and then placed in a vacuum hot-pressed sintering furnace. During the sintering process, the temperature was directly heated from room temperature to 1300°C at a heating rate of 10°C / min, the pressure was maintained at 40 MPa, the pressure holding time was 2 h, and the vacuum degree was 5×10 -4 Pa, and a dense titanium alloy sintered billet is obtained.

[0086] (5) The titanium alloy sintered billet is hot rolled at 750° C. with a deformation amount of 85% to obtain a Ti—Zr alloy plate.

[0087] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.58wt.%, and the particle size of the nitrided fine Ti powder was 2-15μm. The microstructure of the Ti-Zr alloy plate obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix; the distribution of nitrogen in the Ti-Zr alloy plate obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen element was evenly distributed and the content was 0.59wt.%; finally, according to "GBT 228.1-2010 Metallic Material Tensile Test Part 1: Room Temperature Test Method", the Ti-Zr alloy plate obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 1092MPa, the yield strength was 981MPa, the elongation was 17%, and the elastic modulus was 108GPa.

[0088] Example 4

[0089] A method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen is carried out in the following steps:

[0090] (1) Irregular Ti powder with a particle size of 10 to 40 μm (nitrogen content of 0.05 wt.%, purity of 99.5 wt.%) was used as a raw material and loaded into a constant temperature atmosphere jar mill for heating nitriding. The nitriding temperature was 600°C, the nitrogen concentration was 70 vol.%, the speed of the constant temperature atmosphere jar mill was 18 r / min, and the nitriding time was 1 h to obtain nitrided Ti powder.

[0091] (2) The nitriding Ti powder was placed in a ball mill in a glove box, and the ball mill was tightened and placed in a planetary high-energy ball mill for high-energy ball milling. The ball mill speed was 500 r / min, the ball milling time was 2 h, and the ball-to-material ratio was 5:1 to obtain crushed nitriding fine Ti powder. The powder collection and powder loading in this process were carried out in the glove box, and Ar gas protection was used throughout the process.

[0092] (3) Weigh nitriding fine Ti powder and Zr powder (particle size <45 μm, nitrogen content of 0.05 wt.%, purity of 99.3 wt.%) in a mass ratio of nitriding fine Ti powder: Zr powder = 80:20, place the two metal powders in a transition chamber of a glove box under Ar gas environment, and put the two metal powders into a mixing tank in the transition chamber, fill the mixing tank with Ar gas and seal the powders, and then put the mixing tank into a three-dimensional mixer for uniform mixing for 8 hours to obtain a mixed powder.

[0093] (4) The mixed powder was loaded into a hot-pressed graphite mold and then placed in a vacuum hot-pressed sintering furnace. During the sintering process, the temperature was directly heated from room temperature to 1400°C, the heating rate was 10°C / min, the pressure was maintained at 30 MPa, the pressure holding time was 1 h, and the vacuum degree was 5×10 -4Pa, and a dense titanium alloy sintered billet is obtained.

[0094] (5) The titanium alloy sintered billet is hot forged at 900°C with a deformation amount of 90% to obtain a Ti-Zr alloy rod.

[0095] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.63wt.%, and the particle size of the nitrided fine Ti powder was 2-10μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix; the nitrogen distribution in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen distribution was uniform and the content was 0.63wt.%; finally, according to "GBT 228.1-2010 Metallic Material Tensile Test Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 1116MPa, the yield strength was 997MPa, the elongation was 13%, and the elastic modulus was 110GPa.

[0096] Comparative Example 1

[0097] The same as Example 1, except that the flaky Ti powder with a raw material particle size of less than 45 μm used in step (1) is replaced by spherical Ti powder with an average particle size D0=150 μm of the same mass.

[0098] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.35wt.%, and the particle size of the nitrided fine Ti powder was 10-20μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and its SEM photo is as follows: Figure 4 As shown in FIG. 1 , it is found that the Zr element is completely dissolved in the Ti matrix; the distribution of nitrogen in the Ti-Zr alloy rod obtained by energy spectrum analysis step (5) is as follows: Figure 5 As shown, it is found that the nitrogen element is unevenly distributed, local enrichment occurs, and the nitrogen content obtained by test is 0.36wt.%; finally, according to "GBT228.1-2010 Metal Material Tensile Test Part 1: Room Temperature Test Method" the Ti-Zr alloy bar prepared in step (5) is subjected to a tensile test, and the tensile strength of the Ti-Zr alloy is measured to be 964MPa, the yield strength is 875MPa, the elongation is 8%, and the elastic modulus is 107GPa.

[0099] The reason for the sudden decrease in elongation is analyzed as follows: the nitrogen content in the surface of large-sized spherical Ti powder after nitriding is higher than that in the core. The nitrogen element is unevenly distributed in the nitrided fine Ti powder after crushing, resulting in local enrichment of nitrogen in the Ti-Zr alloy after sintering and large deformation. During the tensile deformation process, stress concentration occurs in the nitrogen-rich area, which becomes a crack source, resulting in poor plasticity of the material.

[0100] Comparative Example 2

[0101] The same as Example 1, except that the nitriding temperature in the heating nitriding process of step (1) is 200° C., the nitrogen concentration is 50 vol.%, the speed of the constant temperature atmosphere jar mill is 15 r / min, and the nitriding time is 4 h.

[0102] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.14wt.%, and the particle size of the nitrided fine Ti powder was 2-15μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix; the nitrogen element distribution in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and the energy spectrum diagram showed that the nitrogen element was evenly distributed and the content was 0.19wt.%; finally, according to "GBT 228.1-2010 Metallic Material Tensile Test Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 735MPa, the yield strength was 668MPa, the elongation was 25%, and the elastic modulus was 101GPa.

[0103] The strength of the titanium alloy prepared in this comparative example is relatively low, and the strengthening effect of nitrogen is not fully exerted. The reason is analyzed as follows: the nitriding temperature is too low and the nitrogen concentration is insufficient, which leads to a slow nitriding rate of Ti powder during the nitriding process, and the nitrogen content in the large deformation sample obtained at the end is relatively low, and the nitrogen-enriched strengthening effect is not achieved.

[0104] Comparative Example 3

[0105] The same as Example 1, except that the nitriding temperature in the heating nitriding process of step (1) is 800° C., the nitrogen concentration is 90 vol.%, the speed of the constant temperature atmosphere jar mill is 15 r / min, and the nitriding time is 5 h.

[0106] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 1.06wt.%, and the particle size of the nitrided fine Ti powder was 8-25μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix; the nitrogen element distribution in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen element was evenly distributed and the content was 1.06wt.%; finally, according to "GBT 228.1-2010 Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 1138MPa, the yield strength was 1096MPa, the elongation was 2.3%, and the elastic modulus was 113GPa.

[0107] The reason for the sudden decrease in elongation is analyzed as follows: in a sufficient nitrogen-rich atmosphere, too high a nitriding temperature will cause the Ti powder to nitride faster, significantly increasing the nitrogen content on the surface of the Ti powder, making it difficult to control the nitrogen content in the Ti powder. However, too high a nitrogen content can easily generate metal nitrides, which cannot be removed during sintering and thermal deformation and become defects. They become crack sources during the stretching process, causing premature fracture of the material.

[0108] Therefore, the setting of nitriding parameters must be strictly controlled when heating and nitriding Ti powder.

[0109] Comparative Example 4

[0110] The same as Example 1, except that the ball milling speed in step (2) is 200 r / min, the ball milling time is 2 h, and the ball to material ratio is 5:1.

[0111] The nitrogen content and particle size of the crushed nitrided fine Ti powder obtained in step (2) were tested, and the nitrogen content in the nitrided fine Ti powder was 0.41wt.%, and the particle size of the nitrided fine Ti powder was 15-30μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was not completely dissolved in the Ti matrix, and local enrichment occurred; the nitrogen distribution in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen distribution was uneven, local enrichment occurred, and the content was 0.42wt.%; finally, according to "GBT 228.1-2010 Metal Material Tensile Test Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was 936MPa, the yield strength was 811MPa, the elongation was 12%, and the elastic modulus was 107GPa.

[0112] Analysis shows that the reason for the sudden decrease in elongation is that the ball milling speed is too low, and the nitride film of the nitrided Ti powder is not completely broken, resulting in the nitride film on the surface of the Ti powder hindering the self-diffusion between Ti atoms and the mutual diffusion with Zr atoms during the vacuum hot pressing sintering process. The green body is not sintered densely and leaves residual defects, which are difficult to eliminate during the forging process. Therefore, stress concentration is formed during the stretching process, causing the material to break prematurely.

[0113] Comparative Example 5

[0114] The same as Example 1, except that the ball milling speed in step (2) is 700 r / min, the ball milling time is 4 h, and the ball to material ratio is 5:1.

[0115] The nitrogen content of the crushed nitrided fine Ti powder obtained in step (2) was detected, and the nitrogen content in the nitrided fine Ti powder was measured to be 0.41wt.%, and it was found that the nitrided fine Ti powder after ball milling was welded, and the particle size was measured to be >200μm. The axial microstructure of the Ti-Zr alloy rod obtained in step (5) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix, but there were some residual pores in the Ti matrix; the distribution of nitrogen in the Ti-Zr alloy rod obtained in step (5) was analyzed by energy spectrum analysis, and it was found that the nitrogen element was evenly distributed and the content was 0.43wt.%; finally, according to "GBT 228.1-2010 Metallic Material Tensile Test Part 1: Room Temperature Test Method", the Ti-Zr alloy rod obtained in step (5) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was measured to be 967MPa, the yield strength was 839MPa, the elongation was 4.9%, and the elastic modulus was 107GPa.

[0116] The reason for the sudden decrease in elongation is that the high ball milling speed will cause the crushed Ti powder to weld together, resulting in excessively large particle size and large-sized block Ti powder. During the sintering process, the green body is easily not dense, leaving residual pores, which affects the mechanical properties of the material.

[0117] Therefore, the setting of ball milling parameters must be strictly controlled when high-energy ball milling is performed on nitrided Ti powder.

[0118] Comparative Example 6

[0119] Different from the above-mentioned embodiment and other comparative examples, high nitrogen Ti-20Zr alloy (nitrogen content = 0.6wt.%) was prepared by vacuum arc melting, and the specific steps were as follows:

[0120] (1) The metallurgical raw materials Ti element (nitrogen content of 0.05 wt.%) and Zr element (nitrogen content of 0.03 wt.%) are weighed according to the above-mentioned composition, and the nitrogen element is added by passing nitrogen gas;

[0121] (2) using sandpaper to remove the surface oxide scale of the raw metal Ti and Zr, and using industrial anhydrous ethanol to ultrasonically clean the raw metal for later use;

[0122] (3) Place the raw metal treated in step (2) in a non-consumable vacuum arc furnace for smelting, evacuate the sample chamber, and when the vacuum reaches 5×10 -3 After Pa, nitrogen was filled into the furnace chamber to half the atmospheric pressure to start melting the alloy; after the alloy was melted, the arc was maintained for 60 seconds, and the alloy block was turned over after cooling, and this was repeated 5 times. After the alloy was fully melted and uniformly melted, a vacuum suction casting device was used to suck the alloy into a water-cooled copper mold to obtain a high-nitrogen Ti-20Zr alloy.

[0123] (4) The smelted titanium alloy is hot forged at 900°C with a deformation amount of 90% to obtain a Ti-Zr alloy rod.

[0124] (5) The axial microstructure of the Ti-Zr alloy rod obtained in step (4) was analyzed by scanning electron microscopy, and it was found that the Zr element was completely dissolved in the Ti matrix, but there were still some inclusions dispersed in the Ti matrix. The distribution of nitrogen in the Ti-Zr alloy rod obtained in step (4) was analyzed by energy spectrum analysis, and it was found that the nitrogen element was unevenly distributed and locally enriched near the inclusions, and the content was 0.67wt.%. Finally, according to "GBT 228.1-2010 Tensile Test of Metallic Materials Part 1: Room Temperature Test Method", the Ti-Zr alloy obtained in step (3) was subjected to a tensile test, and the tensile strength of the Ti-Zr alloy was measured to be 1064MPa, the yield strength was 988MPa, the elongation was 7.8%, and the elastic modulus was 106GPa.

[0125] Compared with Example 4, the Ti-Zr alloy prepared by the smelting + large deformation processing method has a strength similar to that of the Ti-Zr alloy prepared by powder metallurgy, but the plasticity is greatly reduced. The reason is analyzed as follows: during the stretching process, stress concentration is easily generated at the nitride inclusions, forming a crack source, causing the material to break prematurely.

[0126] The parameters of each step of the above embodiments and comparative examples are summarized in Table 2:

[0127] Table 2

[0128]

[0129]

[0130] The test data of the above embodiments and comparative examples are summarized in Table 3:

[0131] Table 3

[0132]

[0133]

[0134] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for regulating the mechanical properties of titanium alloy for dental use based on nitrogen, characterized in that: Ti powder is heated and nitrided to obtain nitrided Ti powder; the nitrided Ti powder is subjected to high-energy ball milling to obtain nitrided fine Ti powder; the nitrided fine Ti powder is mixed with Zr powder to obtain mixed powder; the mixed powder is sintered to obtain a titanium alloy sintered blank; the titanium alloy sintered blank is deformed to obtain a titanium alloy.

2. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The particle size of the Ti powder is less than 45 μm, the nitrogen content is less than 0.1 wt.%, and the purity is ≥ 99%; The Ti powder is flaky Ti powder and / or irregular Ti powder.

3. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The heating nitriding temperature is 300-600°C, the time is 1-6 hours, and the nitrogen concentration is 60-90 vol.%; The heating nitriding is carried out in a pot mill; the rotation speed of the pot mill is 10-20r / min.

4. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The rotation speed of the high-energy ball mill is 300-500 r / min, the time is 1-5 hours, and the ball-to-material ratio is 5:1-7:1; the particle size of the nitrided fine Ti powder is ≤20 μm.

5. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The Zr powder has a particle size of <100 μm, a nitrogen content of <0.1 wt.%, and a purity of ≥99%.

6. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The mixing mass ratio of the nitriding fine Ti powder to the Zr powder is 80-95:5-20; and the mixing time is 4-10 hours.

7. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The sintering is vacuum hot pressing sintering, the temperature of vacuum hot pressing sintering is 1000-1500°C, the heating rate is 5-15°C / min, the pressure is 10-50MPa, the holding time is 0.5-4h, the vacuum degree is <10 -3 Pa.

8. The method for regulating the mechanical properties of dental titanium alloy based on nitrogen as claimed in claim 1, characterized in that: The deformation process is selected from rolling, extrusion or forging, the temperature of the deformation process is 800-1100° C., and the deformation amount is 50-90%.

9. A titanium alloy prepared by the method for regulating the mechanical properties of dental titanium alloys based on nitrogen according to any one of claims 1 to 8.

10. Use of the titanium alloy according to claim 9 in preparing oral implants.