High-strength high-plasticity austenite-based dual-phase low-density steel and preparation method thereof
Through the combination of Fe-Mn-Al-C main alloy and Ti-Zr auxiliary alloy, combined with refined technology, high-strength and high-plasticity austenite-based dual-phase low-density steel is prepared, which solves the problems of strength, plasticity and density of traditional materials. The deficiencies in comprehensive performance have improved the performance and application prospects of the material.
Patent Information
- Application Number
- CN202410617740.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2024-10-08
AI Technical Summary
There is still room for improvement in the comprehensive performance of strength, plasticity and density of traditional steel materials. Especially in the fields of aerospace, automobiles and ships, there is an urgent demand for lightweight, high-strength and high-plasticity materials.
Using Fe-Mn-Al-C as the main alloying element, combined with Ti and Zr as auxiliary alloying elements, high-strength and high-plasticity austenite is prepared by precisely controlling the chemical composition and process steps such as smelting, homogenization, heat treatment, etc. Based on dual phase low density steel.
It achieves a good combination of high strength and high plasticity of steel, while maintaining low density, improving corrosion resistance and thermal stability, and has broad industrial application prospects.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metal materials, and specifically relates to a high-strength and high-plasticity austenite-based dual-phase low-density steel and a preparation method thereof. Background Art
[0002] With the advancement of science and technology and the development of industry, the requirements for the performance of metal materials are getting higher and higher. Especially in the fields of aerospace, automobiles, ships, etc., the demand for lightweight, high strength and high plasticity of materials is particularly urgent.
[0003] Although traditional steel materials meet these requirements to a certain extent, their comprehensive performance in strength, plasticity and density still needs to be improved. Therefore, the development of a new type of steel material with high strength, high plasticity and low density is of great significance for improving the performance of industrial products, reducing energy consumption and improving production efficiency. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a high-strength and high-plasticity austenite-based dual-phase low-density steel and a preparation method thereof, which effectively solves the problems raised in the above background.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a high-strength and high-plasticity austenite-based dual-phase low-density steel, comprising the following components in mass percentage: Al: 5-10%, Mn: 10-25%, C: 0.4-0.8%, and the rest are Fe and inevitable trace impurity elements.
[0006] Preferably, Ti and Zr are further included as auxiliary alloying elements, wherein the content of Ti is 0.5-1%, and the content of Zr is 0.2-0.6%.
[0007] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0008] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0009] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0010] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0011] S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0012] S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0013] S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0014] Preferably, in S2, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0015] Preferably, in S4, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0016] Compared with the prior art, the present invention has the following beneficial effects:
[0017] The present invention adopts Fe-Mn-Al-C as the main alloying element, and by precisely controlling its content, the steel achieves a good combination of high strength and high plasticity while maintaining a relatively low density; in addition, the introduction of Ti and Zr as auxiliary alloying elements for composite addition not only improves the corrosion resistance and thermal stability of the steel, but also further optimizes its mechanical properties;
[0018] The Ti-Zr alloyed Fe-Mn-Al-C austenite-based dual-phase low-density steel prepared by this invention is of great significance for improving the performance of industrial products, reducing energy consumption and improving production efficiency, and has broad application prospects. DETAILED DESCRIPTION
[0019] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0020] The invention provides a high-strength and high-plasticity austenite-based dual-phase low-density steel, which comprises the following components in mass percentage: Al: 5-10%, Mn: 10-25%, C: 0.4-0.8%, and the rest are Fe and inevitable trace impurity elements.
[0021] This embodiment further includes Ti and Zr as auxiliary alloying elements, wherein the content of Ti is 0.5-1%, and the content of Zr is 0.2-0.6%.
[0022] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0023] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0024] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0025] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0026] S3: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0027] S4: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0028] S5: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0029] In S2 of this embodiment, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0030] In S4 of this embodiment, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0031] Embodiment 1:
[0032] A high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following components in mass percentage: Al: 5%, Mn: 10%, C: 0.4%, and the rest being Fe and inevitable trace impurity elements.
[0033] This embodiment further includes Ti and Zr as auxiliary alloying elements, wherein the content of Ti is 0.5% and the content of Zr is 0.2%.
[0034] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0035] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0036] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0037] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0038] S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0039] S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0040] S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0041] In S2 of this embodiment, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0042] In S4 of this embodiment, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0043] Embodiment 2:
[0044] A high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following components in mass percentage: Al: 10%, Mn: 25%, C: 0.8%, and the rest being Fe and inevitable trace impurity elements.
[0045] This embodiment further includes Ti and Zr as auxiliary alloying elements, wherein the content of Ti is 0.6% and the content of Zr is 0.3%.
[0046] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0047] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0048] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0049] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0050] S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0051] S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0052] S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0053] In S2 of this embodiment, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0054] In S4 of this embodiment, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0055] Embodiment 3:
[0056] A high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following components in mass percentage: Al: 6%, Mn: 15%, C: 0.6%, and the rest being Fe and inevitable trace impurity elements.
[0057] This embodiment further includes Ti and Zr as auxiliary alloying elements, wherein the content of Ti is 1% and the content of Zr is 0.6%.
[0058] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0059] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0060] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0061] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0062] S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0063] S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0064] S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0065] In S2 of this embodiment, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0066] In S4 of this embodiment, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0067] Embodiment 4:
[0068] A high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following components in mass percentage: Al: 8%, Mn: 20%, C: 0.7%, and the rest being Fe and inevitable trace impurity elements.
[0069] This embodiment further includes Ti and Zr as auxiliary alloying elements, wherein the content of Ti is 0.8% and the content of Zr is 0.5%.
[0070] A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel comprises the following steps:
[0071] S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio;
[0072] S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed;
[0073] S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment.
[0074] S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape;
[0075] S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material;
[0076] S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
[0077] In S2 of this embodiment, during smelting, possible volatilization and burning loss in the production process are taken into consideration and appropriate compensation is made for some elements.
[0078] In S4 of this embodiment, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.
[0079] The austenite-based dual-phase low-density steel prepared in the above embodiment has the following properties:
[0080]
[0081]
[0082] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A high-strength, high-plasticity austenite-based dual-phase low-density steel, It is characterized in that The invention comprises the following components in mass percentage: Al: 5-10%, Mn: 10-25%, C: 0.4-0.8%, and the rest are Fe and inevitable trace impurity elements.
2. A high-strength and high-plasticity austenite-based dual-phase low-density steel according to claim 1, It is characterized in that Ti and Zr are also included as auxiliary alloying elements, wherein the content of Ti is 0.5-1%, and the content of Zr is 0.2-0.6%.
3. A method for preparing high-strength and high-plasticity austenite-based dual-phase low-density steel, It is characterized in that The following steps are involved: S1: Raw material preparation: accurately weigh Fe, Mn, Al, C, Ti, Zr and other raw materials according to the above chemical composition ratio; S2: Melting, which is carried out in an induction melting furnace, a converter or an electric furnace. Fe is first added as the base material, and then Al, Mn and C are gradually added. The temperature and time are strictly controlled during the melting process to ensure that the elements are fully integrated and evenly distributed; S3: Homogenization: the ingot is heated to 1100°C and kept at this temperature for several hours for homogenization treatment. S4: continuous casting and deformation, the refined molten steel is continuously cast to obtain the initial steel billet, which is then hot forged and hot rolled, cooled to room temperature by water cooling, and finally cold rolled to obtain the required steel size and shape; S5: Heat treatment, heat treatment of the rolled steel, including annealing at 900°C and cooling to room temperature by water cooling, to further optimize the structure and performance of the material; S6: Inspection and post-processing: strict quality inspection of the heat-treated steel to ensure that its performance meets the design requirements, followed by post-processing operations such as cutting and grinding to obtain the final product.
4. A method for preparing a high-strength and high-plasticity austenite-based dual-phase low-density steel according to claim 3, It is characterized in that In S2, during smelting, possible volatilization and burning losses in the production process are taken into consideration and appropriate compensation is made for some elements.
5. The method for preparing a high-strength and high-plasticity austenite-based dual-phase low-density steel according to claim 3, It is characterized in that In S4, the hot forging temperature ranges from 800 to 1100°C, and the hot rolling temperature ranges from 800 to 1100°C.