High-strength wear-resistant corrosion-resistant steel with excellent plasticity for photovoltaic bracket and manufacturing method of high-strength wear-resistant corrosion-resistant steel
By using high-strength, wear-resistant, and corrosion-resistant steel with optimized chemical composition and processes, the problems of insufficient corrosion resistance and wear resistance in photovoltaic bracket materials have been solved, achieving excellent plasticity and formability of high-strength photovoltaic brackets, and ensuring the durability and safety of photovoltaic brackets.
Patent Information
- Application Number
- CN202410857972.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing photovoltaic support materials are insufficient in terms of corrosion resistance and wear resistance. In particular, the plasticity and formability of steel used in thin-gauge, high-strength photovoltaic supports are poor. Furthermore, existing technologies are either costly or have complex processes, making it difficult to meet the long-term durability requirements of photovoltaic supports.
High-strength wear-resistant and corrosion-resistant steel with a specific chemical composition ratio, including a reasonable combination of elements such as C, Si, Mn, Cr, Cu, Sb, Ti, Mo, and Ce, and through precise smelting, rolling and cooling processes, fine Mo2Si3 hard phase and Mo2C3 particles are formed, which improves the hardness and plasticity of the steel plate. The addition of rare earth Ce avoids copper embrittlement defects and improves the formability.
It achieves excellent plasticity and formability of high-strength photovoltaic bracket steel, significantly improves wear resistance and atmospheric corrosion resistance, ensures the durability of photovoltaic brackets in bending processing and windy and sandy environments, and reduces production costs.
Smart Images

Figure BDA0004918544770000071 
Figure BDA0004918544770000082 
Figure BDA0004918544770000083
Abstract
Description
Technical Field
[0001] The invention belongs to the field of corrosion-resistant steel for photovoltaic brackets, and relates to high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity and a manufacturing method thereof. Background Art
[0002] As an important supporting device in the photovoltaic power generation system, the performance of the photovoltaic bracket directly affects the service life of the photovoltaic power station. Since the photovoltaic bracket is exposed to the atmospheric environment for a long time, it will cause different degrees of corrosion to the bracket, thus affecting the durability of the bracket. Especially for photovoltaic power stations built in the Gobi desert and windy and sandy areas, the photovoltaic bracket must also withstand the abrasion of wind and sand. Therefore, the corrosion resistance and wear resistance of the material must be considered. At the same time, the photovoltaic bracket needs to go through a series of complex deformation processes during the processing and manufacturing process, so it is also required that the manufactured material has excellent plasticity and forming properties to avoid bending cracks in the material during the deformation process.
[0003] At present, most materials used to manufacture photovoltaic brackets are processed from low-grade steel coils or lightweight profiles and then galvanized. However, the production process of hot-dip galvanized products is complicated and the galvanizing process has a heavy impact on the environment. Weathering steel is an ideal material for processing photovoltaic brackets due to its corrosion resistance. However, domestic weathering steel for photovoltaic brackets often only considers its atmospheric corrosion resistance and ignores the wear resistance required for the bracket to be in service. At the same time, as the trend of weathering steel for photovoltaic brackets develops towards thin specifications and high strength, the requirements for its ductility and formability are gradually increasing. Therefore, it is an urgent need for the development of the photovoltaic industry to develop a high-strength steel for photovoltaic brackets that has high corrosion resistance, high wear resistance and excellent formability.
[0004] Prior to the present invention,
[0005] The invention patent "A high-strength weathering steel for photovoltaic brackets and its preparation method" with publication number CN 115786822 B has the following components: C: 0.05% to 0.07%, Si: 0.30% to 0.40%, Mn: 0.70% to 1.00%, P: ≤0.025%, S: ≤0.005%, Als: 0.020% to 0.040%, Cu: 0.25% to 0.35%, Cr: 0.55% to 0.75%, Ni: 0.15% to 0.30%, Nb: 0.030% to 0.050%, Ti: 0.070% to 0.090%, N: ≤0.005%, Ca: 0.0005% to 0.0020%, and the rest is Fe and impurities. Precious metal Ni is added in this invention, and the content of this element is relatively high. The addition of Ni will increase the cost. Moreover, the invention does not mention the specific impact on wear resistance, and the corrosion resistance is only predicted using the theoretical parameter I. The specific corrosion resistance index of the invented steel is not explained, so its actual wear resistance and corrosion resistance are unknown.
[0006] The invention patent "Antimony-containing weathering steel for low-cost 650MPa photovoltaic bracket and its preparation method" with publication number CN 116121668 A has the following components: C: ≤0.08%, Si: 0.35%~0.50%, Mn: 0.40%~0.60%, P: 0.08%~0.12%, S: ≤0.010%, Cu: 0.25%~0.40%, Cr: 0.75%~1.00%, Ti: 0.065%~0.105%, N: ≤0.0050%, Sb: 0.05%~0.07%, and the rest is Fe and impurities. The high content of Cu in this invention will not only increase the cost, but also cause cracks on the edge of the steel plate; this invention improves the corrosion resistance of the invention steel by adding P, but the increase of P is prone to element segregation, which will seriously reduce the plasticity of the steel plate, thus adversely affecting the deformation of the photovoltaic bracket in the later processing. In addition, the invention does not mention the specific impact on wear resistance, and the corrosion resistance is only predicted using the theoretical parameter I. The specific corrosion resistance index of the invented steel is not explained, so its actual wear resistance and corrosion resistance are unknown.
[0007] The invention patent "A corrosion-resistant, wear-resistant steel plate and its preparation method" with publication number CN112159934A has the following components: C: 0.14%~0.22%, Si: 0.10%~1.00%, Mn: 0.1%~1.0%, P: less than 0.015%, S: less than 0.005%, Cr: 3.00%~6.00%, Ni: 0.00%~1.50%, Mo: 0.00%~0.80%, Als: 0.02%~0.06%, B: 0.0008%~0.005%, Ca: 0.0015%~0.0040%, wherein Ca / S≥1, and the rest is Fe and impurities. The Cr element added in this invention has a high content, which increases the difficulty of smelting; and this invention improves the corrosion resistance by adding Cr, but does not clarify the corrosion resistance index, and the corrosion environment targeted is acidic conditions; this invention obtains a hard phase martensitic structure through a quenching + tempering process to improve the wear resistance of the invention steel, and the process flow is relatively complicated.
[0008] The invention patent "Coal-water wear and corrosion resistant steel plate for railway coal transport vehicles and its manufacturing method" with publication number CN107653423B has the following components: C: 0.01%~0.15%, Si: 0.10%~0.50%, Mn: 0.20%~1.0%, P≤0.020%, S≤0.010%, Cu: 0.20%~0.60%, Ni: 0.50%~1.5%, Cr: 0.20%~2.0%, Sb: 0.030%~0.10%, Mo: 0%~0.25%, Nb: 0%~0.05%, V: 0%~0.05%, Ti: 0%~0.10%, B: 0%~0.005%, and the rest are Fe and impurities; and C, Cr, and Ni must satisfy 1.6%≤12C+Cr / Ni≤2.8%. The invention controls the content of C, Cr, and Ni to meet 1.6%≤12C+Cr / Ni≤2.8%, and the wear and corrosion rate relative to Q450NQR1 is 20% to 30%. However, the types and contents of precious metal elements such as Cu, Ni, Nb, and V added in the invention are relatively large, which will cause a significant increase in production costs and is not conducive to its promotion; the invention does not describe the corrosion resistance of the product, and the wear resistance and corrosion resistance of the steel of the invention are aimed at its performance in the coal-water corrosion environment, which is very different from the corrosion environment of the photovoltaic bracket. Summary of the invention
[0009] The purpose of the present invention is to provide a high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity and a manufacturing method thereof. The high-strength steel for photovoltaic brackets not only has excellent plasticity and forming properties, but also has excellent wear resistance and atmospheric corrosion resistance, solving the problem of insufficient plasticity and lack of wear resistance of thin-gauge, high-strength photovoltaic bracket steel in the prior art.
[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0011] The present invention provides a high-strength wear-resistant and corrosion-resistant steel for a photovoltaic bracket with excellent plasticity, wherein the chemical composition is C: 0.074%-0.094%, Si: 0.39%-0.57%, Mn: 0.91%-1.16%, P: ≤0.016%, S: ≤0.006%, Cr: 1.03%-1.27%, Cu: 0.16%-0.24%, Sb: 0.106%-0.126%, Ti: 0.051%-0.071%, Mo: 0.20%-0.32%, Ce: 0.0168%-0.0188%, Als: 0.050%-0.073%, wherein Si / Mo is controlled at 1.2-2.9, and the balance is Fe and unavoidable impurities.
[0012] The present invention selects the above alloy element types and contents because:
[0013] C: As one of the key elements to ensure the strength and hardness of the material. In the present invention, C mainly improves the strength of the steel plate by solid solution strengthening and precipitation strengthening. When added in conjunction with Mo, a hard phase Mo2C3 can be generated inside the grains to improve the hardness and wear resistance of the steel. However, excessive C will deteriorate the plasticity and forming properties of the steel plate. In the present invention, the content of C is limited to 0.074% to 0.094%.
[0014] Si: As one of the important elements for improving corrosion resistance, strength and hardness. Si is easy to be enriched on the surface of the steel plate, thereby forming a dense SiO2 oxide protective film on the surface of the product that is tightly bonded to the matrix, which can effectively inhibit the penetration of corrosive media. When added in combination with Mo, it can form Mo2Si3 hard phase particles with free Mo in the steel. By controlling the final rolling temperature and the coiling temperature, it is easy to disperse and precipitate micron-level (40-70μm) hard phase Mo2Si3 particles near the grain boundary or inside the grain, which can effectively improve the hardness and wear resistance of the steel. However, too high Si content will not only have an adverse effect on the surface quality, but also deteriorate the performance of the steel due to the generation of large-sized Mo2Si3 particles. Therefore, the content of Si in the present invention is limited to 0.39% to 0.57%. In addition, the content of Si and Mo determines the type of Si-Mo and the state of the precipitated particles. In order to obtain more dispersed precipitated phase particles, Si / Mo is controlled at 1.2 to 2.9.
[0015] Mn: One of the main strengthening elements in steel, it can improve the strength of steel plate through solid solution strengthening. At the same time, Mn in the present invention, as an important austenitizing stabilizing element, can expand the austenite phase region, has the effect of improving the stability of the retained austenite in the steel, and can improve the plasticity of the material. Therefore, in order to ensure and improve the strength and plasticity of the material, the content of Mn in the present invention is set to 0.91% to 1.16%
[0016] P: Although P is one of the alloying elements that plays a role in solid solution strengthening and significantly improves the corrosion resistance, when its content is too high, it is easy to segregate at the grain boundary and reduce the welding performance, plasticity and toughness of the steel plate. In the steel of the present invention, P is controlled below 0.016%.
[0017] S: It is a harmful impurity element in steel, which is easy to form defects such as segregation and inclusion, and will deteriorate the impact toughness and hot working performance of the steel plate. However, if the S content is controlled too low, the smelting cost will increase. Therefore, in the present invention, the S content should be controlled below 0.006%.
[0018] Cr: Mainly improves the strength of steel by solid solution strengthening, and this element can significantly improve the tensile limit of steel. Its contribution to improving tensile strength is higher than yield strength, and it can effectively reduce the yield strength ratio of the material. At the same time, this element is also the main corrosion-resistant element, and it is often enriched in the rust layer. It is not only easy to form a dense oxide film on the surface of the steel plate, but also forms a dense Cr-Cu compound protective rust layer on the surface of the substrate with the Cu element, which can significantly inhibit the penetration of corrosive media, thereby achieving a double-layer corrosion resistance effect, and can replace part of the corrosion resistance of Cu. However, when its content is high, it will not only deteriorate the welding performance of the steel plate but also increase the difficulty of smelting. Therefore, the Cr content in the present invention is controlled to be 1.03% to 1.27%.
[0019] Cu: One of the important corrosion-resistant elements. This element is often enriched in the rust layer, which can effectively improve the permeability of the corrosive medium, and it is easy to form a dense Cu-P compound protective rust layer with the P element on the surface of the substrate, which can further inhibit the penetration of the corrosive medium. At the same time, this element is often dissolved in Fe to form a substitutional solid solution, which has a solid solution strengthening effect, thereby improving the strength of the steel plate. However, when the Cu content is too high, it not only causes an increase in cost, but also easily causes "copper brittleness" defects on the edge of the steel plate in the absence of Ni elements. Therefore, in the present invention, the rare earth Ce element is added to make it dispersed and combined with a heating process to avoid the occurrence of "copper brittleness" defects. The present invention limits its content range to 0.16% to 0.24%.
[0020] Ti: A strong C and N compound-forming element, an important element for improving strength. During the heating process of the steel plate, it often forms Ti-N compounds with N to inhibit the growth of austenite grains and achieve the purpose of grain refinement; it forms fine carbides and nitrides or carbonitrides with C and N, and then precipitates fine compounds during the cooling and coiling of the steel plate, playing a precipitation strengthening role. The present invention limits its range to 0.051% to 0.071%.
[0021] Sb: An effective element for improving the corrosion resistance and wear resistance of steel plates. This element easily forms a dense oxide film on the surface of the substrate, improving the passivation ability of the steel plate. By adding it in combination with P, Cu, and Cr, it is synergistically enriched in the rust layer, forming a dense Sb-P-Cu-Cr composite protective rust layer that is tightly bonded to the substrate, which can further hinder the invasion of corrosive media. In addition, the Sb3O4 hard phase formed by this element inside the substrate precipitates along the grain boundaries during cooling and coiling, which can further improve the wear resistance of the steel plate. In the present invention, the content of Sb is controlled to be 0.106% to 0.126%.
[0022] Mo: There are three main forms of existence in steel. One part is dissolved in iron to form a substitutional solid solution, which improves the yield strength of the steel; one part forms a Mo-C hard phase Mo2C3 with the free C in the steel, which can significantly improve the hardness and wear resistance of the steel; and a small part is segregated at the grain boundary; when Mo is added in combination with the rare earth Ce, the strong affinity of Ce can reduce the segregation of Mo at the grain boundary. Ce promotes the uniform precipitation of the Mo2C3 hard phase and inhibits its aggregation and growth, which can further improve the wear resistance of the steel plate; especially when added in combination with Si, it can form Mo2Si3 hard phase particles with the free Si in the steel. By controlling the final rolling temperature and the coiling temperature, micron-level (40-70μm) hard phase Mo2Si3 particles will be dispersed and precipitated near the grain boundary or inside the grain, which greatly improves the hardness and wear resistance of the steel. In order to better exert the synergistic wear-resistant effect of Si and Mo, the present invention limits Si / Mo to 1.2-2.9. However, when the Mo content is too high, its segregation degree at the grain boundary will increase, and the plasticity, toughness and welding performance of the steel will be deteriorated. The Mo content is controlled at 0.20%-0.32%.
[0023] Als: An important deoxidizing element that can purify the molten steel into a low-oxygen environment so that the rare earth will not react with the excessive oxygen in the molten steel after being added, and the solid solution effect of the rare earth can be fully exerted. A large part of the role of this element is to be added in conjunction with the addition of rare earth. The present invention limits its range to 0.050% to 0.073%.
[0024] Ce: (1) As an effective deoxidizing and desulfurizing element, it can purify molten steel and improve the mechanical properties of the product; it can change the shape and type of inclusions, reduce the potential difference between inclusions and the matrix, reduce the tendency of electrochemical corrosion caused by inclusions, and effectively improve the corrosion resistance of the steel plate; (2) It has the function of dispersing Cu, which can avoid the occurrence of "copper brittleness" defects on the one hand, and improve the utilization rate of Cu on the other hand, thereby increasing the ratio of protective phase α-FeOOH / γ-FeOOH, improving the stability of the rust layer, and further improving the corrosion resistance of the steel plate; (3) It improves the segregation of Mo, promotes the uniform precipitation of hard phases Mo2C3 and Mo2Si3, and inhibits the aggregation and growth of these phases, thereby improving the wear resistance of the steel plate; (4) The addition of RE elements helps to inhibit the decomposition of residual austenite and the precipitation of carbides, which can significantly improve the plasticity and forming properties of the steel plate, and facilitate the later processing of the material such as bending. The present invention limits its range to 0.0168% to 0.0188%.
[0025] The present invention also provides a method for manufacturing high-strength, wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity. The method obtains wear-resistant and atmospheric corrosion-resistant steel containing the above-mentioned chemical components through pre-desulfurization of molten iron, top and bottom blowing of converter, LF refining outside the furnace, slab continuous casting, ingot heating, hot rolling, laminar cooling and coiling, and specifically includes the following contents.
[0026] Smelting: firstly, the molten iron is subjected to a desulfurization pretreatment so that the S in the molten iron after desulfurization is ≤0.002%. A top and bottom composite blowing process is adopted, and the converter tapping temperature is 1646-1661°C. Then, the molten iron is fed into the LF furnace for heating and component fine-tuning, and then Si-Ca wire feeding treatment is carried out to further reduce the O and S contents, and ensure that the free O content in the steel should be controlled below 3.6ppm; 7-9 minutes before the end of the vacuum treatment in the LF furnace, 20% Ce-Fe rare earth alloy 1.87-2.09kg / ton of steel is added to the LF furnace, and then argon weak blowing (argon flow rate 110-130NL / min, pressure 0.18-0.31MPa) and stirring are carried out, and the weak blowing time is 4.1-6.1min to ensure that the inclusions are fully floated and denatured.
[0027] Slab continuous casting: During the slab continuous casting, protective slag is used to protect the molten steel throughout the process to prevent the molten steel from being exposed to the air. The thickness of the continuous casting billet is 210-230mm. Since the rare earth element Ce in the invention steel has a strong affinity, it is easy to form a large number of rare earth inclusions with the O and S elements in the steel, affecting the fluidity of the molten steel. Therefore, the pulling speed is controlled to 1.32-1.52m / min during casting; and in order to reduce the center segregation of the continuous casting billet, the superheat is controlled between 20-23℃ during casting, and electromagnetic stirring, dynamic soft pressure and other technologies are used at the same time.
[0028] Ingot heating: One of the main ways to improve the strength of the steel plate in the present invention is microalloy solid solution strengthening, especially when Si and Mo elements are added in combination. In order to ensure that Si, Mo and other alloy elements are fully dissolved, the ingot is heated to 1270-1296°C. The steel of the present invention is copper-containing steel. Usually, Cu and Ni elements should be added in combination to suppress the occurrence of "copper brittleness" defects. However, in order to reduce costs, the present invention does not add precious metal Ni, but avoids the occurrence of "copper brittleness" defects of copper-containing steel by formulating a reasonable heating process. Therefore, in order to avoid the occurrence of "copper brittleness" defects caused by the precipitation of low-melting-point element Cu on the surface of the steel plate, the atmosphere of the heating furnace is set to a reducing atmosphere with an air-fuel ratio between 1.6 and 2.0. When the heating temperature is below 1105°C, slow heating is required, and the heating rate is controlled at 6.2 to 8.3°C / min to ensure uniform temperature inside and outside the billet; when the temperature is above 1105°C, rapid heating is required, and the heating rate is controlled at 16.5 to 18.5°C / min; since the longer the heating time, the more conducive it is for Cu to diffuse along the austenite grain boundary, and the more likely it is to produce "copper brittleness" defects, the furnace time is controlled to be ≤200min, preferably 172 to 195min, with the soaking section holding time being 32 to 47min.
[0029] Rolling: Rough rolling and finishing rolling are two-stage temperature-controlled rolling. Rough rolling adopts high temperature and large reduction. The final rolling temperature of rough rolling is 1104-1139℃. The cumulative reduction rate of rough rolling stage is 82.1%-85.3%. The higher cumulative reduction can not only press the defects in the ingot, but also form more dislocations by increasing deformation, thereby improving the strength of the material by dislocation strengthening. The start rolling temperature of finishing rolling is 1085℃-1113℃. In order to eliminate the adverse effects of dislocation strengthening on plasticity in the rough rolling stage and ensure that the hard phases of Mo2C3 and Mo2Si3 are fully precipitated, a higher final rolling temperature is set for this purpose, and the final rolling temperature of finishing rolling is set to 932-948℃; in order to ensure the straightness and precision of the finished steel plate, the reduction rate of the last rolling of finishing rolling is controlled at 15.8%-16.7%. And during the rolling process, the rolling convexity target is controlled at 34-41μm.
[0030] After finishing rolling, laminar cooling is performed in two stages. In the first stage, the steel is cooled to 746-766 (this temperature range belongs to the ferrite transformation range) at a cooling rate of 18-25°C / s, and air-cooled for 8-10s. In this stage, sufficient soft ferrite structure can be obtained and Mo2C3 and Mo2Si3 phases can be inoculated so that they are easy to precipitate and grow, so as to ensure the plasticity and wear resistance of the steel plate; then the second stage is cooled at a cooling rate of 29-39°C / s, and the steel is cooled to 594-614°C for coiling. In this stage, sufficient hard bainite can be generated to ensure the strength performance of the product. And this coiling temperature has a good effect on refining grains and inhibiting the coarsening of Mo2C3 and Mo2Si3 precipitation phases.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] Through precise control of the composition and tissue proportion, the yield strength of the 1.8-4.0mm wear-resistant and corrosion-resistant steel coil for photovoltaic brackets produced by the above chemical composition and rolling process is 633-655MPa, the tensile strength is 812-842MPa, the elongation is greater than 34%, and the yield strength ratio is 0.77-0.79, with excellent plasticity and forming properties; through the control of hard phase precipitates and their sizes, the surface hardness of the invention steel is 220-224HBW, and the wear rate relative to Q345B is 28.1%-29.2%; through the reasonable combination of corrosion-resistant elements, in the rapid corrosion evaluation test simulating the C4 grade atmospheric environment, the corrosion rate of the invention steel relative to Q345B is 29.74%-32.48%. The present invention overcomes the shortcomings of the prior art and produces thin-gauge, high-strength weathering steel for photovoltaic brackets that has both excellent plasticity and forming properties and excellent wear resistance and atmospheric corrosion resistance, ensuring that the photovoltaic brackets will not have defects such as cracks during bending and deformation, and will be safe and durable when used in windy and sandy areas. DETAILED DESCRIPTION
[0033] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] The present invention is described in more detail below through examples.
[0035] The composition of the steel of the embodiment of the present invention is shown in Table 1, the main process parameters of smelting and continuous casting of the steel of the embodiment of the present invention are shown in Table 2, the heating process parameters of the steel of the embodiment of the present invention are shown in Table 3, the rolling and coiling process parameters of the steel of the embodiment of the present invention are shown in Table 4, the various properties of the steel of the embodiment of the present invention are shown in Table 5, the microstructure of the steel of the embodiment of the present invention is shown in Table 6, and the results of the circumferential immersion corrosion test of the steel of the embodiment of the present invention are shown in Table 7.
[0036] Table 1 Composition of steel according to the present invention (wt%)
[0037]
[0038]
[0039] Table 2 Main process parameters of steel smelting and continuous casting in the embodiment of the present invention
[0040]
[0041] Table 3 Heating process of steel in the embodiment of the present invention
[0042]
[0043] Table 4 Main process parameters of rolling and cooling of steel in the embodiment of the present invention
[0044]
[0045] Table 5 Test results of various performance indicators of the embodiment
[0046]
[0047] Table 6 Microstructure of steel according to the present invention
[0048]
[0049] It can be seen from Table 5 that the yield strength of the example steels of the present invention is between 633 and 655 MPa, the tensile strength is between 812 and 842 MPa, the elongation is greater than 34%, and the yield strength ratio is between 0.77 and 0.79, indicating that the example steels have excellent plasticity and forming properties; the hardness value of the example steels is between 220 and 224 HBW.
[0050] The wear resistance test in Table 5 was conducted on a wet rubber wheel abrasive wear tester. The sample size was 57.0mm×25.5mm×6.0mm. The wear test was conducted in accordance with "JB / T 7705-1995 Loose Abrasive Wear Test Method Rubber Wheel Method". The test results show that the wear rate of the example steel relative to Q345B is between 28.1% and 29.2%, which shows that the example steel has higher wear resistance.
[0051] The results in Table 6 show that the structure of the invented steel is composed of ferrite + bainite + a small amount of pearlite, the structure is uniform and fine, and fine Mo2Si3 hard phase is precipitated in the structure, among which Mo2Si3 with a size range of 40 to 70 μm accounts for 86.4% to 88.4%. This level of precipitated phase is beneficial to improving the wear resistance of the invented steel.
[0052] In order to simulate the corrosion situation in the C4 grade atmospheric environment, the invention steel was subjected to a 72-hour periodic immersion rapid corrosion evaluation test according to the test method specified in TB / T 2375-1993. Table 7 shows the corrosion resistance comparison results of the embodiment steel of the invention and the comparative steel. It can be seen from Table 7 that the corrosion resistance of the embodiment steel of the invention is significantly better than that of the comparative steel Q345B.
[0053] Table 7 Comparison results of rapid corrosion test of steel according to the present invention and comparative steel
[0054]
[0055] It is to be noted that the above embodiments are only for illustrating the technical concept and features of the present invention, and are not intended to limit the present invention. Any equivalent replacement or modification that does not deviate from the essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A high-strength, wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity, characterized in that: The chemical composition of the steel is as follows by weight: C: 0.074% ~ 0.094%, Si: 0.39% ~ 0.57%, Mn: 0.91% ~ 1.16%, P: ≤ 0.016%, S: ≤ 0.006%, Cr: 1.03% ~ 1.27%, Cu: 0.16% ~ 0.24%, Sb: 0.106% ~ 0.126%, Ti: 0.051% ~ 0.071%, Mo: 0.20% ~ 0.32%, Ce: 0.0168% ~ 0.0188%, Als: 0.050% ~ 0.073%, wherein Si / Mo is controlled at 1.2 ~ 2.9, and the balance is Fe and unavoidable impurities.
2. The high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 1 is characterized in that: The metallographic structure of the steel is ferrite + bainite + a small amount of pearlite, with the proportion of ferrite being 29.3% to 31.1%, the proportion of bainite being 59.5% to 60.5%, and the ferrite grain size being ≥ 10.5; fine Mo2Si3 hard phase is precipitated in the structure, among which the proportion of Mo2Si3 with a size range of 40 to 70 μm is 86.4% to 88.4%.
3. The high-strength, wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 1 is characterized in that: The yield strength of the steel is between 633 and 655 MPa, the tensile strength is between 812 and 842 MPa, the elongation is greater than 34%, and the yield strength ratio is 0.77 to 0.79; the surface hardness of the steel is 220 to 224 HBW, and the wear rate relative to Q345B is 28.1 to 29.2%.
4. The high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 1 is characterized in that: In the rapid corrosion evaluation test simulating the C4 grade atmospheric environment, the corrosion rate of steel was 0.998~1.09g / m 2 .h, the corrosion rate relative to Q345B is 29.74%~32.48%.
5. The high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 1 is characterized in that: The thickness of the steel plate is 1.8 to 4.0 mm.
6. A method for manufacturing high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity as claimed in any one of claims 1 to 5, comprising smelting, slab continuous casting, billet heating, rolling, laminar cooling and coiling, characterized in that: The ingot is heated to 1270-1296°C, the air-fuel ratio is between 1.6 and 2.0, the heating rate is controlled at 6.2-8.3°C / min when the heating temperature is below 1105°C; the heating rate is controlled at 16.5-18.5°C / min when the heating temperature is above 1105°C; the furnace time is controlled to be ≤200min; the rolling adopts two-stage controlled rolling of rough rolling and finishing rolling, the final rolling temperature of rough rolling is 1104-1139°C, the cumulative reduction rate of rough rolling stage is 82.1%-85.3%; finishing rolling The starting rolling temperature is 1085℃~1113℃, the finishing rolling temperature is 932~948℃, the reduction rate of the last finishing rolling is controlled at 15.8%~16.7%, and the rolling convexity target is controlled at 34~41μm; after finishing rolling, two-stage laminar cooling is adopted. In the first stage, the steel is cooled to 746~766℃ at a cooling rate of 18~25℃ / s, air cooled for 8~10s, and then cooled to 594~614℃ for coiling at a cooling rate of 29~39℃ / s in the second stage.
7. The method for manufacturing high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 6, characterized in that: During smelting, the molten iron is first pre-treated with desulfurization. After desulfurization, the S in the molten iron is ≤0.002%. The top and bottom composite blowing process is adopted, and the converter tapping temperature is 1646-1661°C. After that, Si-Ca wire feeding treatment is carried out to control the free O content in the steel below 3.6ppm. 20% Ce-Fe rare earth alloy 1.87-2.09kg / ton of steel is added to the LF furnace 7-9min before the end of the vacuum treatment in the LF furnace, and then argon weak blowing is carried out.
8. The method for manufacturing high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 7, characterized in that: The flow rate of argon weak blowing is 110-130NL / min, the pressure is 0.18-0.31MPa, and the weak blowing time is 4.1-6.1min.
9. The method for manufacturing high-strength wear-resistant and corrosion-resistant steel for photovoltaic brackets with excellent plasticity according to claim 6, characterized in that: The ingot heating time in the furnace is 172 to 195 minutes, of which the soaking time is 32 to 47 minutes.
Citation Information
Patent Citations
Coal-water abrasion and corrosion resistant steel plate for railway coal transport vehicle and manufacturing method thereof
CN107653423A
550MPa-grade wear-corrosion-resistant steel and manufacturing method thereof
CN114686763A
450MPa-grade sulfuric acid dew point corrosion resistant rare earth steel and manufacturing method thereof
CN115652208A
Short-process high-strength ultra-atmospheric-corrosion-resistant hot-rolled strip steel and production method thereof
CN117089769A
High-corrosion-resistance 670MPa-grade hot-rolled weather-resistant steel plate for photovoltaic support and preparation method of hot-rolled weather-resistant steel plate
CN117488209A
Cited By
High-corrosion-resistance wear-resistant steel for railway wagon and manufacturing method of high-corrosion-resistance wear-resistant steel
CN120138507A
High-strength corrosion-resistant steel bar and production method thereof
CN120290990A
Abrasion-resistant high-strength steel for power transmission tower and preparation method thereof
CN121250244A