Coaxial piezoelectric fiber preparation device and method based on magnetic field arrangement

By introducing magnetic field alignment technology into coaxial wet spinning technology, piezoelectric ceramic particles are oriented and arranged, which solves the problem of unstable piezoelectric output caused by disordered dipole directions in piezoelectric ceramics and polymer composites. The performance of piezoelectric fibers is significantly improved and is suitable for the application of flexible electronic devices.

CN118745654APending Publication Date: 2024-10-08XI AN JIAOTONG UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410758787.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Existing piezoelectric ceramics and piezoelectric polymer composite materials lead to disordered dipole directions of piezoelectric ceramic particles during the doping process, which limits the stability and efficiency of piezoelectric output, making it difficult to be widely used in the field of flexible electronic devices. .

Method used

Coaxial wet spinning technology based on magnetic field alignment is used to directionally arrange the magnetically sensitive piezoelectric ceramic particles in the piezoelectric functional layer of the fiber by introducing an external magnetic field, thereby improving the pressure sensitivity of the fiber in the alignment direction, thereby improving the piezoelectricity. performance.

Benefits of technology

Through magnetic field alignment technology, the dipole orientation is consistent, significantly improving the piezoelectric output performance, achieving higher electromechanical conversion efficiency and stability, and is suitable for applications in wearable devices and flexible sensors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745654A_ABST
    Figure CN118745654A_ABST
Patent Text Reader

Abstract

The invention discloses a coaxial piezoelectric fiber preparation device and method based on magnetic field arrangement. The coaxial piezoelectric fiber preparation device comprises a fiber conveying roll, and the fiber conveying roll conveys a carbon fiber bundle to be collected by a fiber collecting roll through a coaxial needle tube, a magnetic field arrangement device and a water bath; the coaxial needle tube comprises a sleeve, the upper end of the sleeve is connected with a first needle head, the lower end of the sleeve is connected with a second needle head, the side of the second needle head is connected with a third needle head, a spinning solution is injected into the third needle head, and the spinning solution is composed of a piezoelectric polymer and magnetic induction piezoelectric ceramic particles distributed in the piezoelectric polymer; the magnetic field arrangement device comprises a parallel magnetic field space formed by a magnetic field north pole plate and a magnetic field south pole plate, and the parallel magnetic field space is used for arranging magnetic induction piezoelectric ceramic particles distributed in the piezoelectric polymer; a water bath solution is injected into the water bath tank, and the arranged fibers enter the water bath solution to remove a solvent to obtain coaxial piezoelectric fibers; the coaxial piezoelectric fiber is steered by a roller, and is collected and dried by a fiber collecting roll; the pressure sensitivity of the fibers in the arrangement direction is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of piezoelectric materials, and in particular relates to a device and method for preparing coaxial piezoelectric fibers based on magnetic field arrangement. Background Art

[0002] Piezoelectric materials refer to crystalline materials that, when subjected to external forces, separate charges will appear at both ends to generate voltage. This phenomenon is called the piezoelectric effect, which can realize the mutual conversion between mechanical energy and electrical energy. Using this characteristic of piezoelectric materials, various sensor elements and micro-nano energy devices can be made.

[0003] Barium titanate (BT) and lead zirconate titanate (PZT) are typical piezoelectric ceramic materials with advantages such as low price, easy synthesis and high piezoelectric coefficient. They have been widely used. However, their high molding temperature, difficulty in making complex shapes and high brittleness limit their application in the rapidly developing field of flexible electronic devices. Boron nitride (BN) piezoelectric ceramic is a new type of piezoelectric material with many advantages: first, it has excellent piezoelectric properties, showing high piezoelectric coefficient and excellent piezoelectric stability; second, boron nitride has good mechanical properties and chemical stability, can work stably in harsh environments such as high temperature and high pressure, and has a long service life; in addition, compared with lead titanate, boron nitride has lower toxicity and environmental friendliness.

[0004] Polyvinylidene fluoride (PVDF), as a polymer piezoelectric material, has attracted much attention due to its advantages such as flexibility, low density and sensitive response. PVDF is a semi-crystalline polymer with five crystal phases, among which the β crystal phase has a higher dipole moment and exhibits a significant piezoelectric effect; the α crystal phase is the most stable crystal phase of PVDF, but it has no piezoelectric properties and can be transformed into the β crystal phase through polarization. Binary and ternary copolymers of PVDF, such as polyvinylidene fluoride-trifluoroethylene (P(VDF-TrFE)) and polyvinylidene fluoride-trifluoroethylene-hexafluoropropylene (P(VDF-TrFE-HFP)), are more likely to exhibit the β crystal phase at room temperature. PVDF-based piezoelectric materials overcome the difficulties of ceramic piezoelectric materials such as hardness and brittleness and difficulty in processing, and have broad application prospects; however, the piezoelectric effect of pure PVDF-based polymers is much lower than that of traditional ceramic materials, and the electromechanical conversion efficiency is not high, which limits its application.

[0005] In order to comprehensively solve the brittleness problem of ceramic piezoelectric materials and the efficiency problem of polymer piezoelectric materials, the common practice is to compound ceramic materials with polymers to combine the advantages of both. In previous reports, researchers compounded piezoelectric ceramics with piezoelectric polymers to obtain materials that are both flexible and have a high piezoelectric effect (Nano Energy, 2017, 33: 462-468.), and made some progress; however, since piezoelectric ceramics need to be dispersed during the doping process to form disordered random directions, the dipole directions of the dispersed piezoelectric ceramic particles are also disordered, and the resulting piezoelectric charge separation may cancel each other out, thereby limiting its total piezoelectric output.

[0006] Wet spinning technology is one of the common methods for preparing fibers. Its main process is to squeeze the polymer solution or melt from the blank through an aperture controller or a rotating component to form fibers. In wet spinning technology, solvents or solutions are usually used to dissolve the polymer material so that it can flow more easily during the spinning process and quickly solidify to form fibers after spinning. Coaxial wet spinning is an improved version of wet spinning technology. Its main feature is the use of a coaxial spinning structure during the spinning process. The structure is usually two concentric cylindrical spinning holes, where the outer hole is used to inject the polymer solution or melt, and the inner hole is used to inject auxiliary fluids, such as air or solvents; or insert fibers inside, so that the polymer material is coaxially attached to the surface of the internal fiber to form a coaxial fiber with a core-sheath structure. Coaxial wet spinning technology has higher flexibility and controllability in the fiber preparation process, and can prepare fiber products with different morphologies, structures and properties.

[0007] In summary, the current use of piezoelectric ceramics and piezoelectric polymers to prepare piezoelectric fibers has the disadvantage of unstable piezoelectric output. Summary of the invention

[0008] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a device and method for preparing coaxial piezoelectric fibers based on magnetic field arrangement. On the basis of coaxial wet spinning, the magneto-inductive piezoelectric material in the piezoelectric functional layer of the fiber is directional arranged by introducing an external magnetic field, thereby improving the pressure sensitivity of the fiber in the arrangement direction and obtaining fibers with higher piezoelectric properties. The prepared coaxial piezoelectric fibers can be used as power sources for wearable devices, highly sensitive flexible sensors, or implanted into fiber-reinforced composite materials to form a sensing network to realize the stress distribution monitoring function of the composite materials.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A coaxial piezoelectric fiber preparation device based on magnetic field arrangement includes a fiber delivery roll, the fiber delivery roll delivers a carbon fiber bundle through a coaxial needle tube, a magnetic field arrangement device, and a water bath, and is collected by a fiber collection roll;

[0011] The coaxial needle tube includes a sleeve, the upper end of the sleeve is connected to a first needle, the lower end of the sleeve is connected to a second needle, the first needle and the second needle are used to limit the carbon fiber bundle; the side of the second needle is connected to a third needle, the third needle is injected into the spinning solution, the spinning solution is composed of a piezoelectric polymer and magnetically inductive piezoelectric ceramic particles distributed in the piezoelectric polymer;

[0012] The magnetic field arrangement device includes a parallel magnetic field space formed by a magnetic field north pole plate and a magnetic field south pole plate, and the parallel magnetic field space arranges magnetically inductive piezoelectric ceramic particles distributed in the piezoelectric polymer;

[0013] The water bath tank is filled with a water bath solution, and the arranged fibers enter the water bath solution, and the solvent of the spinning solution is removed to obtain the coaxial piezoelectric fiber; the coaxial piezoelectric fiber is turned by a roller, collected by a fiber collection roll and dried.

[0014] The diameter of the carbon fiber bundle is 1k, 3k, 6k, 12k, etc., and fibers of different diameters can be obtained by selecting different k numbers; the models of the carbon fiber are T300, T700, T800, etc., depending on the cost requirements and strength requirements.

[0015] The spinning solution is prepared by dissolving piezoelectric polymer PVDF powder in solvent N,N-dimethylacetamide (DMAc) to obtain PVDF solution, and then dispersing magnetically inductive piezoelectric ceramic particles boron nitride nanosheets (BNNS) in the PVDF solution.

[0016] The piezoelectric polymer PVDF is composed of any one or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE), polyvinylidene fluoride-trifluoroethylene-hexafluoropropylene P (VDF-TrFE-HFP), depending on the specific cost and functional requirements; the solvent is any organic solvent that can dissolve PVDF material but not dissolve boron nitride material, including but not limited to N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAc); the specific form of the magnetically inductive piezoelectric ceramic particle boron nitride is any one of boron nitride nanotubes (BNNT) and boron nitride nanosheets (BNNS), depending on the specific cost and functional requirements.

[0017] The water bath solution is deionized water, or other liquids that can quickly dissolve the organic solvent in the spinning solution.

[0018] The fiber collecting roll is provided with an electric driving device, which can be turned on to allow the carbon fiber bundle to be wound continuously.

[0019] A method for preparing a device using a coaxial piezoelectric fiber based on magnetic field alignment comprises the following steps:

[0020] The first step is to install the carbon fiber bundle on the coaxial piezoelectric fiber preparation device based on magnetic field arrangement, that is, from the fiber delivery roll through the coaxial needle tube, the magnetic field arrangement device, the water bath to the fiber collection roll;

[0021] Step 2: Place the water bath solution in a water bath tank so that the liquid surface completely submerges the carbon fiber bundle;

[0022] Step 3: Prepare the spinning solution: add 1g of piezoelectric polymer, namely PVDF powder, into 20mL of N,N-dimethylacetamide (DMAc) solvent, and stir magnetically for 3h at 60℃; add 0.2g of magnetically inductive piezoelectric ceramic particles, namely boron nitride nanosheets (BNNS), into the PVDF solution, stir evenly, and then disperse ultrasonically for 2h;

[0023] Step 4: Use a syringe to absorb the spinning solution and place it on the electric-controlled microfluidic pump; set the electric-controlled microfluidic pump to propel the solution at a speed of 0.02-0.2 mL / min, and inject the spinning solution into the coaxial needle tube through the third needle;

[0024] Step 5: When the spinning solution fills the second needle, turn on the electric drive device of the fiber collection roll to start the preparation of the coaxial piezoelectric fiber; after the preparation is completed, put the coaxial piezoelectric fiber collected by the fiber collection roll into a vacuum drying oven for drying, and polarize the coaxial piezoelectric fiber after drying.

[0025] In the fifth step, the pulling speed of the electric drive device of the fiber collection roll is 10-100 mm / min.

[0026] The drying conditions in the fifth step are a temperature of 100-120° C. and a drying time of more than 1 hour.

[0027] The direction of the polarization electric field in the fifth step needs to be consistent with the arrangement direction of the magnetic field arrangement device. Considering the polarization effect and avoiding breakdown, the polarization electric field strength is 10-40V / μm.

[0028] Compared with the prior art, the advantages of the present invention are as follows: the present invention adds a magnetic field arrangement process on the basis of the existing coaxial wet spinning process, the preparation process is simple, and no additional cost is added; the present invention adopts a method of mixing piezoelectric polymer and piezoelectric ceramic nanoparticles, which has higher piezoelectric performance than a single piezoelectric polymer; the present invention arranges the magnetically inductive piezoelectric ceramic nanoparticles inside the piezoelectric functional layer through a magnetic field arrangement method, thereby making the dipole orientation consistent, further improving the piezoelectric output. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1It is a schematic diagram of a coaxial piezoelectric fiber preparation device based on magnetic field arrangement according to an embodiment.

[0030] Figure 2 It is a schematic diagram of the fiber cross section before and after the magnetic field arrangement of the magnetic field arrangement device of the embodiment.

[0031] Figure 3 It is a comparison diagram of the piezoelectric properties of the piezoelectric fibers before and after the magnetic field arrangement under the conditions of the embodiment. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the accompanying drawings and embodiments.

[0033] Reference Figure 1 and Figure 2 , a coaxial piezoelectric fiber preparation device based on magnetic field arrangement, comprising a fiber delivery roll 1, the fiber delivery roll 1 delivers a carbon fiber bundle 2 through a coaxial needle tube, a magnetic field arrangement device, and a water bath 8 and is collected by a fiber collection roll 11;

[0034] The coaxial needle tube includes a sleeve 4, the upper end of the sleeve 4 is connected to a first needle 3-1, and the lower end of the sleeve 4 is connected to a second needle 3-2, and the first needle 3-1 and the second needle 3-2 limit the carbon fiber bundle 2; the second needle 3-2 is laterally connected to a third needle 3-3, and the third needle 3-3 injects a spinning solution 5, and the spinning solution 5 is composed of a piezoelectric polymer 13 and magnetically inductive piezoelectric ceramic particles 12 distributed in the piezoelectric polymer 13;

[0035] The magnetic field arrangement device includes a parallel magnetic field space formed by a magnetic field north pole plate 6 and a magnetic field south pole plate 7, and the parallel magnetic field space arranges the magnetically inductive piezoelectric ceramic particles 12 distributed in the piezoelectric polymer 13;

[0036] The water bath tank 8 is filled with a water bath solution 9, and the arranged fibers enter the water bath solution 9 to remove the solvent of the spinning solution 5 to obtain coaxial piezoelectric fibers; the coaxial piezoelectric fibers are turned by rollers 10, collected by fiber collection rolls 11 and dried.

[0037] In this embodiment, the carbon fiber bundle 2 is of 1k and T300 type.

[0038] Reference Figure 1 , a method for preparing a device using a coaxial piezoelectric fiber based on magnetic field alignment, comprising the following steps:

[0039] The first step is to install the carbon fiber bundle 2 on the coaxial piezoelectric fiber preparation device based on magnetic field arrangement, that is, from the fiber delivery roll 1 through the coaxial needle tube, the magnetic field arrangement device, the water bath 8 to the fiber collection roll 11;

[0040] Step 2: placing a water bath solution 9 in a water bath tank 8, with the liquid surface completely immersing the carbon fiber bundle 2; in this embodiment, the water bath solution 9 is deionized water;

[0041] Step 3: Prepare spinning solution 5: add 1g of piezoelectric polymer 13, i.e., PVDF powder, into 20mL of solvent N,N-dimethylacetamide (DMAc), and stir magnetically for 3h at 60°C to fully dissolve; add 0.2g of magnetically inductive piezoelectric ceramic particles 12, i.e., boron nitride nanosheets (BNNS), into the PVDF solution, stir evenly, and then disperse ultrasonically for 2h to fully disperse the BNNS;

[0042] Step 4: use a 10 mL syringe to absorb a certain amount of spinning solution 5, and place it on the electric-controlled microfluidic pump; set the electric-controlled microfluidic pump to propel the solution at a speed of 0.06 mL / min, and inject the spinning solution 5 into the coaxial needle tube through the third needle 3-3;

[0043] Step 5: When the spinning solution 5 fills the second needle 3-2, the electric drive device of the fiber collection roll 11 is turned on to start the preparation of the coaxial piezoelectric fiber; after the preparation is completed, the coaxial piezoelectric fiber collected by the fiber collection roll 11 is placed in a vacuum drying oven for drying to remove residual deionized water; after drying, the coaxial piezoelectric fiber is polarized;

[0044] In this embodiment, the pulling speed of the coaxial piezoelectric fiber is 55 mm / min; the temperature of the vacuum drying oven is set at 100° C., and the drying time is 2 h; the direction of the polarization electric field is consistent with the arrangement direction of the magnetic field, and the polarization electric field strength is 20 V / μm.

[0045] In this embodiment, under the same load conditions, the piezoelectric signal output comparison diagram of the piezoelectric fiber before and after the magnetic field arrangement is as follows: Figure 3 As shown, the piezoelectric output before the magnetic field arrangement is about 0.17V, and the piezoelectric output after the magnetic field arrangement is about 0.82V, which indicates that the magnetic field arrangement improves the output performance of the piezoelectric fiber by 4.8 times.

Claims

1. A coaxial piezoelectric fiber preparation device based on magnetic field arrangement, comprising a fiber delivery roll, characterized in that: The fiber delivery roll delivers the carbon fiber bundle through the coaxial needle tube, magnetic field arrangement device, and water bath, and is collected by the fiber collection roll; The coaxial needle tube includes a sleeve, the upper end of the sleeve is connected to a first needle, the lower end of the sleeve is connected to a second needle, the first needle and the second needle are used to limit the carbon fiber bundle; the side of the second needle is connected to a third needle, the third needle is injected into the spinning solution, the spinning solution is composed of a piezoelectric polymer and magnetically inductive piezoelectric ceramic particles distributed in the piezoelectric polymer; The magnetic field arrangement device includes a parallel magnetic field space formed by a magnetic field north pole plate and a magnetic field south pole plate, and the parallel magnetic field space arranges magnetically inductive piezoelectric ceramic particles distributed in the piezoelectric polymer; A water bath solution is filled in the water bath, and the arranged fibers enter the water bath solution, and the solvent of the spinning solution is removed to obtain the coaxial piezoelectric fiber; The coaxial piezoelectric fibers are deflected by rollers, collected by a fiber collection roll and dried.

2. The device according to claim 1, characterized in that: The diameters of the carbon fiber bundles are 1k, 3k, 6k, and 12k, and fibers of different diameters can be obtained by selecting different k numbers; the models of the carbon fibers are T300, T700, and T800.

3. The device according to claim 1, characterized in that The spinning solution is prepared by dissolving piezoelectric polymer PVDF powder in solvent N,N-dimethylacetamide (DMAc) to obtain PVDF solution, and then dispersing magnetically inductive piezoelectric ceramic particles boron nitride nanosheets (BNNS) in the PVDF solution.

4. The device according to claim 3, characterized in that: The piezoelectric polymer PVDF is any one or more of polyvinylidene fluoride PVDF, polyvinylidene fluoride-trifluoroethylene P (VDF-TrFE), polyvinylidene fluoride-trifluoroethylene-hexafluoropropylene P (VDF-TrFE-HFP); the solvent is any organic solvent that can dissolve PVDF material but not boron nitride material, including N,N-dimethylformamide (DMF) and N,N-dimethylacetamide (DMAc); the specific form of the magnetically inductive piezoelectric ceramic particle boron nitride is any one of boron nitride nanotubes (BNNT) and boron nitride nanosheets (BNNS).

5. The device according to claim 1, characterized in that: The water bath solution is deionized water, or other liquids that can quickly dissolve the organic solvent in the spinning solution.

6. The device according to claim 1, characterized in that: The fiber collecting roll is provided with an electric driving device, which can be turned on to allow the carbon fiber bundle to be wound continuously.

7. A method for preparing a coaxial piezoelectric fiber based on magnetic field alignment according to any one of claims 1 to 6, characterized in that: The following steps are involved: The first step is to install the carbon fiber bundle on the coaxial piezoelectric fiber preparation device based on magnetic field arrangement, that is, from the fiber delivery roll through the coaxial needle tube, the magnetic field arrangement device, the water bath to the fiber collection roll; Step 2: Place the water bath solution in a water bath tank so that the liquid surface completely submerges the carbon fiber bundle; Step 3: Prepare the spinning solution: add 1g of piezoelectric polymer, namely PVDF powder, into 20mL of N,N-dimethylacetamide (DMAc) solvent, and stir magnetically for 3h at 60℃; add 0.2g of magnetically inductive piezoelectric ceramic particles, namely boron nitride nanosheets (BNNS), into the PVDF solution, stir evenly, and then disperse ultrasonically for 2h; Step 4: Use a syringe to draw the spinning solution and place it on an electrically controlled microfluidic pump; The electric-controlled microfluidic pump is set to propel the solution at a speed of 0.02-0.2 mL / min, and the spinning solution is injected into the coaxial needle tube through the third needle; Step 5: When the spinning solution fills the second needle, the electric drive device of the fiber collection roll is turned on to start the preparation of the coaxial piezoelectric fiber; After the preparation is completed, the coaxial piezoelectric fibers collected in the fiber collection roll are placed in a vacuum drying oven for drying, and after drying, the coaxial piezoelectric fibers are polarized.

8. The method according to claim 7, characterized in that: In the fifth step, the pulling speed of the electric drive device of the fiber collection roll is 10-100 mm / min.

9. The method according to claim 7, characterized in that: In the fifth step, the drying conditions are a temperature of 100-120° C. and a drying time of more than 1 hour.

10. The method according to claim 7, characterized in that: In the fifth step, the direction of the polarization electric field needs to be consistent with the arrangement direction of the magnetic field arrangement device, and the polarization electric field strength is 10-40V / μm.

Citation Information

Cited By

  • Multi-layer coaxial piezoelectric sensing fiber, preparation method thereof and flexible wearable fabric

    CN119824577A

  • Multilayer coaxial piezoelectric sensing fiber and method of making same, flexible wearable fabric

    CN119824577B