Fluorine-free super-hydrophilic-high oleophobic fabric and preparation method thereof

By using a compound of polydimethylsiloxane and long-chain alkyl compounds to replace traditional long-chain perfluoroalkyl compounds, fluorine-free super-hydrophilic-high oleophobic fabrics are prepared, which solves the environmental hazard problem of traditional fabrics. Efficient oil-water separation is achieved and fabric safety is improved.

CN118745667APending Publication Date: 2024-10-08JIAXING UNIV
View PDF 0 Cites -1 Cited by

Patent Information

Application Number
CN202410990613.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

Long-chain perfluoroalkyl compounds commonly used in existing hydrophilic-oleophobic fabrics pose hazards to human health and the environment, and are difficult to degrade, leading to environmental pollution.

Method used

A complex of polydimethylsiloxane and long-chain alkyl compounds is used as the oleophobic component, and traditional long-chain perfluoroalkyl compounds are replaced by fluorine-free chemical components to prepare fluorine-free super-hydrophilic-high oleophobic fabrics , modifying the fabric surface through solution dipping and heating drying processes.

Benefits of technology

The preparation of fluorine-free super-hydrophilic-high oleophobic fabric is achieved, which reduces the harm to the human body and the environment. The process is simple and easy to operate, and the fabric has excellent oil-repellent performance and firmness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118745667A_ABST
    Figure CN118745667A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: preparing a glycerol propoxy triglycidyl ether solution, preparing a polydimethylsiloxane and long-chain alkyl compound solution, mixing the solutions according to a ratio, heating and stirring, immersing the fabric into the solution, heating and drying to obtain the fluorine-free super-hydrophilic and high-oleophobic fabric. The fluorine-free super-hydrophilic and high-oleophobic fabric is obtained. The fabric prepared by the invention adopts a surface treatment method of the fluoride-free super-hydrophilic-high oleophobic fabric, after the solution is prepared, a one-step dip coating process is adopted, and the method is simple and easy to operate. A fluorine-free chemical is used as a hydrophilic-oleophobic coating, so that the safety to a human body and the environment is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fabric modification, and particularly relates to a fluorine-free super hydrophilic-high oleophobic fabric and a preparation method thereof. Background Art

[0002] Hydrophilic-oleophobic fabrics have a wide range of applications in many fields, and these applications are mainly based on their unique surface properties, that is, they can strongly attract water molecules and repel oil molecules. In recent years, the phenomenon of oil pollution in water sources has received widespread attention, and oil-water separation has become an increasingly urgent issue. Hydrophobic-oleophilic fabrics have been widely used for oil-water separation, but such fabrics are easily contaminated, and the density of oil is generally less than that of water, resulting in the water layer easily blocking the penetration of the oil layer. In contrast, hydrophilic-oleophobic fabrics can effectively solve this problem. Under the action of gravity, water penetrates the fabric, while the oil is blocked by the fabric, thereby achieving the purpose of oil-water separation. In the field of self-cleaning, hydrophilic-oleophobic fabrics contaminated with oil stains are immersed in water. Due to the oleophobic nature, the oil layer and the fiber will not adhere firmly. Its superhydrophilicity allows water to penetrate into the interface between the fiber and the oil layer. The infiltrated water layer will easily peel off the oil stains from the fiber surface to achieve the purpose of cleaning.

[0003] Although more and more researchers are involved in the research of hydrophilic-oleophobic fabrics, there are still some unresolved issues: long-chain perfluoroalkyl compounds (greater than or equal to eight carbon atoms) are often used as oleophobic components in hydrophilic-oleophobic coatings, and these substances are harmful to human health and the environment. Studies have shown that long-chain perfluoroalkyl compounds, especially fluorocarbon chemicals with a perfluoroalkyl chain length of eight carbon atoms or more, are difficult to degrade during use, have a long half-life in the body, are bioaccumulative, and will accumulate in the human body and cause harm, so they are being banned worldwide. Summary of the invention

[0004] In order to solve the above technical problems, the present invention adopts a complex of polydimethylsiloxane and a long-chain alkyl compound as the oleophobic component in the hydrophilic-oleophobic compound, and aims to reduce the harm to human health and the environment through the fluorine-free chemical composition.

[0005] The technical solution adopted by the present invention is: a method for preparing a fluorine-free super hydrophilic-high oleophobic fabric, comprising the following steps:

[0006] 1) selecting an organic solvent to prepare a glyceryl propoxy triglycidyl ether solution;

[0007] 2) selecting an organic solvent to prepare a solution of polydimethylsiloxane and a long-chain alkyl compound;

[0008] 3) mixing the solution prepared in step 1) with the solution prepared in step 2) in a certain proportion, and then heating and stirring;

[0009] 4) soaking the fabric in the solution prepared in step 3) for a period of time, then taking it out, heating and drying the fabric to obtain a fluorine-free super hydrophilic and highly oleophobic fabric.

[0010] As a preferred embodiment of the above technical solution, the organic solvent in step 1) and the organic solvent in step 2) are respectively one or more of toluene, ethanol, acetone, tetrahydrofuran or N,N-dimethylformamide.

[0011] As a preferred embodiment of the above technical solution, the concentration of the glycerol propoxy triglycidyl ether solution is 1-2wt%; the concentration of the polydimethylsiloxane and long-chain alkyl compound solution is 2-4wt%; the weight-average molecular weight of the polydimethylsiloxane is 2500, and the viscosity is 100mPa·s; the long-chain alkyl compound is one or more of octadecylamine, octadecyltrimethoxysilane, hexadecylamine, and hexadecyltrimethoxysilane.

[0012] As a preferred embodiment of the above technical solution, the weight ratio of polydimethylsiloxane to the long-chain alkyl compound in the polydimethylsiloxane and long-chain alkyl compound solution is 1:1-2.

[0013] As a preferred embodiment of the above technical solution, in step 3), the volume ratio of the glycerol propoxy triglycidyl ether solution to the polydimethylsiloxane and long-chain alkyl compound solution is 1:2.

[0014] As a preferred embodiment of the above technical solution, the heating temperature during the heating and stirring process of step 3) is 50-70°C, the heating and drying temperature of step 4) is 120-140°C, and the fabric soaking time is 1-3 minutes.

[0015] As a preferred embodiment of the above technical solution, the fabric is one of cotton, polyester and wool.

[0016] The fluorine-free super hydrophilic-high oleophobic fabric is prepared by adopting the above preparation method.

[0017] The beneficial effects of the present invention are:

[0018] (1) The present invention provides a surface treatment method for fluorine-free super hydrophilic and highly oleophobic fabrics. After the solution is prepared, a one-step dipping coating process is adopted. The method is simple and easy to operate.

[0019] (2) The polydimethylsiloxane and long-chain alkyl compound solution are modified on the fabric surface, which has the effect of synergistically reducing the surface energy.

[0020] (3) Conventional hydrophilic-oleophobic coatings often use long-chain perfluoroalkyl compounds (chain length greater than or equal to eight carbon atoms) as oleophobic components, and these substances are harmful to human health and the environment. The present invention uses fluorine-free chemicals as hydrophilic-oleophobic coatings, which improves safety for the human body and the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The photos are of the original cotton cloth and the fabric prepared in Example 1;

[0022] Figure 2 The following are scanning electron microscope images of the original cotton cloth and the fabric prepared in Example 1. DETAILED DESCRIPTION

[0023] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Embodiment 1:

[0025] (1) using toluene as a solvent, preparing a 1 wt % glyceryl propoxy triglycidyl ether solution;

[0026] (2) using toluene as a solvent, preparing a 2 wt % polydimethylsiloxane and octadecylamine solution, wherein the polydimethylsiloxane:octadecylamine=1:1;

[0027] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 50° C. in a sealed state;

[0028] (4) Immerse the cotton cloth in the solution prepared in step (3) for 1 minute, then take out the cloth, place it in an oven and heat it at 120° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0029] Embodiment 2:

[0030] (1) using acetone as a solvent, preparing a 2 wt % glyceryl propoxy triglycidyl ether solution;

[0031] (2) using acetone as a solvent, preparing a 3 wt % polydimethylsiloxane and hexadecylamine solution, wherein the polydimethylsiloxane: hexadecylamine = 1:2;

[0032] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 70° C. in a sealed manner;

[0033] (4) Immerse the polyester fabric in the solution prepared in step (3) for 3 minutes, then take out the fabric, place it in an oven and heat it at 140° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0034] Embodiment 3:

[0035] (1) using ethanol as a solvent, preparing a 2 wt % glyceryl propoxy triglycidyl ether solution;

[0036] (2) using ethanol as a solvent, preparing a 4 wt % polydimethylsiloxane and octadecyltrimethoxysilane solution, wherein the polydimethylsiloxane:octadecyltrimethoxysilane=1:2;

[0037] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 60° C. in a sealed container;

[0038] (4) Immerse the wool cloth in the solution prepared in step (3) for 2 minutes, then take out the cloth, place it in an oven and heat it at 130° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0039] Embodiment 4:

[0040] (1) using tetrahydrofuran as a solvent, preparing a 1 wt % glyceryl propoxy triglycidyl ether solution;

[0041] (2) using tetrahydrofuran as a solvent, preparing a 4 wt % polydimethylsiloxane and hexadecyltrimethoxysilane solution, wherein the polydimethylsiloxane: hexadecyltrimethoxysilane = 1:1;

[0042] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 50° C. in a sealed state;

[0043] (4) Immerse the cotton cloth in the solution prepared in step (3) for 1 minute, then take out the cloth, place it in an oven and heat it at 120° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0044] Embodiment 5:

[0045] (1) using N,N-dimethylformamide as a solvent, preparing a 2 wt % glyceryl propoxy triglycidyl ether solution;

[0046] (2) using N,N-dimethylformamide as a solvent, preparing a 2 wt % polydimethylsiloxane and octadecylamine solution, wherein the polydimethylsiloxane:octadecylamine=1:1;

[0047] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 70° C. in a sealed manner;

[0048] (4) Immerse the wool cloth in the solution prepared in step (3) for 3 minutes, then take out the cloth, place it in an oven and heat it at 140° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0049] Comparative Example 1:

[0050] (1) using toluene as a solvent, preparing a 1 wt % glyceryl propoxy triglycidyl ether solution;

[0051] (2) using toluene as a solvent to prepare a 2 wt % polydimethylsiloxane solution;

[0052] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 50° C. in a sealed state;

[0053] (4) Immerse the cotton cloth in the solution prepared in step (3) for 1 minute, then take out the cloth, place it in an oven and heat it at 120° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0054] Comparative Example 2:

[0055] (1) using toluene as a solvent, preparing a 1 wt % glyceryl propoxy triglycidyl ether solution;

[0056] (2) using toluene as a solvent to prepare a 2 wt % octadecylamine solution;

[0057] (3) mixing the solution prepared in step (1) with the solution prepared in step (2) in a volume ratio of 1:2, and then heating and stirring at 50° C. in a sealed state;

[0058] (4) Immerse the cotton cloth in the solution prepared in step (3) for 1 minute, then take out the cloth, place it in an oven and heat it at 120° C. to dry it, thereby obtaining a fluorine-free super hydrophilic-high oleophobic fabric.

[0059] The wetting properties and air permeability of the original cotton cloth and the fabrics prepared in Examples 1-5 and Comparative Examples 1-2 are shown in Table 1.

[0060] Table 1:

[0061]

[0062] The fastness test of the fabric prepared in Example 1 is shown in Table 2.

[0063] Table 2:

[0064]

[0065] Note:

[0066] (1) Washing test: Tested according to AATCC61-2006 No.2A standard;

[0067] (2) Wear resistance test: Tested according to ASTM D4966 standard;

[0068] (3) Acid solution test: Place the prepared fabric in a pH = 1 aqueous solution for 1 hour, rinse with clean water and dry;

[0069] (4) Alkaline solution test: The prepared fabric was placed in an aqueous solution of pH = 12 for 1 hour, rinsed with clean water and dried.

[0070] The photos of the original cotton cloth and the fabric obtained in Example 1 are as follows Figure 1 As shown;

[0071] The scanning electron microscope images of the original cotton cloth and the fabric obtained in Example 1 are as follows: Figure 2 shown.

[0072] From the above data, we can see that:

[0073] (1) The test results in Table 1 show that the original cotton cloth has the characteristics of super hydrophilicity and super oleophilicity; the fabrics prepared in Examples 1-5 have super hydrophilicity and high oleophobicity. The oil contact angle to hexadecane reaches 137-140°, and according to the standard GB / T19977-2014, its oil repellency is grade 6, indicating excellent oil repellency. The water contact angle is 0°, indicating excellent hydrophilicity.

[0074] (2) The oil contact angles of Comparative Examples 1-2 are lower than those of Examples 1-5 to a certain extent, indicating that the combined solution of polydimethylsiloxane and long-chain alkyl compounds modified on the fabric surface has the effect of synergistically reducing the surface energy.

[0075] (3) From Table 2, it can be seen that the super-hydrophilic-high oleophobic fabric prepared in Example 1 still maintains the super-hydrophilic-high oleophobic properties and has a certain degree of firmness after being damaged by external washing, abrasion and acid-base corrosion.

[0076] It is worth mentioning that the technical features such as the oven and scanning electron microscope involved in the patent application of this invention should be regarded as the prior art. The specific structure, working principle and possible control method and spatial layout method of these technical features can be selected by conventional methods in the field, and should not be regarded as the inventive point of this patent. This patent will not be further elaborated.

[0077] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in this field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in this technical field through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the existing technology should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a fluorine-free super hydrophilic-high oleophobic fabric, characterized in that: The following steps are included: 1) selecting an organic solvent to prepare a glyceryl propoxy triglycidyl ether solution; 2) selecting an organic solvent to prepare a solution of polydimethylsiloxane and a long-chain alkyl compound; 3) mixing the solution prepared in step 1) with the solution prepared in step 2) in a certain proportion, and then heating and stirring; 4) soaking the fabric in the solution prepared in step 3) for a period of time, then taking it out, heating and drying the fabric to obtain a fluorine-free super hydrophilic and highly oleophobic fabric.

2. The method for preparing a fluorine-free super hydrophilic-high oleophobic fabric according to claim 1, characterized in that: The organic solvent in step 1) and the organic solvent in step 2) are respectively one or more of toluene, ethanol, acetone, tetrahydrofuran or N,N-dimethylformamide.

3. The method for preparing the fluorine-free super hydrophilic-high oleophobic fabric according to claim 2, characterized in that: The concentration of the glycerol propoxy triglycidyl ether solution is 1-2wt%; the concentration of the polydimethylsiloxane and long-chain alkyl compound solution is 2-4wt%; the weight-average molecular weight of the polydimethylsiloxane is 2500 and the viscosity is 100mPa·s; the long-chain alkyl compound is one or more of octadecylamine, octadecyltrimethoxysilane, hexadecylamine, and hexadecyltrimethoxysilane.

4. The method for preparing the fluorine-free super hydrophilic-high oleophobic fabric according to claim 3, characterized in that: The weight ratio of polydimethylsiloxane to the long-chain alkyl compound in the polydimethylsiloxane and long-chain alkyl compound solution is 1:1-2.

5. The method for preparing the fluorine-free super hydrophilic-high oleophobic fabric according to claim 4, characterized in that: In the step 3), the volume ratio of the glyceryl propoxy triglycidyl ether solution to the polydimethylsiloxane and long-chain alkyl compound solution is 1:

2.

6. The method for preparing the fluorine-free super hydrophilic-high oleophobic fabric according to claim 5, characterized in that: The heating temperature in the heating and stirring process of step 3) is 50-70° C., the heating and drying temperature in step 4) is 120-140° C., and the fabric soaking time is 1-3 minutes.

7. The method for preparing the fluorine-free super hydrophilic-high oleophobic fabric according to claim 1, characterized in that: The fabric is one of cotton, polyester and wool.

8. Fluorine-free super hydrophilic-high oleophobic fabric, characterized in that: The method is prepared according to any one of claims 1 to 7.