Hydrophobic oleophylic insulation paper, and preparation method and application thereof
By forming a composite coating of polytetrafluoroethylene, perfluoroalkyl phosphate and carbon black on the transformer insulating paper, the problems of hydrophobic and lipophilic properties, insulation aging and insufficient self-healing properties of the insulating paper are solved, achieving a more efficient Insulating properties and extended service life.
Patent Information
- Application Number
- CN202410731955.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-06
- Publication Date
- 2024-10-08
AI Technical Summary
Existing transformer insulation paper cannot balance good hydrophobicity and lipophilicity, insulation aging performance and self-healing performance. Moreover, self-healing temperature after physical damage is high and energy consumption is large, and the repair effect needs to be improved.
It uses hydrophobic and lipophilic insulating paper including base paper, organic coating and carbon black coating. The organic coating is composed of polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyltriethoxysilane. , the carbon black coating is located outside the organic coating, and forms a hydrophobic and lipophilic insulating paper through a specific soaking and drying process.
It significantly improves the hydrophobic and lipophilic ability and self-healing performance of the insulating paper, delays the aging speed of the insulating paper, enhances the mechanical and electrical properties, solves the problem of insulation aging, and has the ability to self-repair after physical damage.
Smart Images

Figure CN118745685A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of transformers, and in particular to a hydrophobic and oleophilic insulating paper, a preparation method and application thereof. Background Art
[0002] Electricity is the foundation of national economic development, and transformers are the core of the power transmission process. Their safety and stability are directly related to the reliability of power supply in the power grid. The transformers used in the current power system can be divided into dry type and oil-immersed type according to the insulating medium. The oil-immersed transformer adopts the "oil-paper" liquid-solid composite insulation mechanism, which has simple process and low cost, and is widely used in power systems of various voltage levels. However, during the long-term operation of the transformer, the oil-paper insulation system will be continuously affected by temperature and electromagnetic fields, and its heat dissipation, insulation and arc extinguishing performance will decrease to varying degrees. At the same time, the insulating paper wrapped around the transformer will also become brittle and fall off, resulting in serious safety hazards and even major accidents such as insulation breakdown. Although the deteriorated insulating oil can be solved by replacing new oil or filtering, the insulating paper wrapped with the transformer is difficult to replace, and the aging phenomenon is irreversible. Therefore, studying the insulating paper that is difficult to replace in the insulation of the transformer and improving its various performances has great engineering practical significance for reducing the replacement frequency of the insulating paper and thus extending the service life of the transformer. It is also of great significance for improving the voltage level of the power grid and maintaining the safe and stable operation of the power grid.
[0003] The existing insulating paper is affected by various stress factors during long-term operation, and its mechanical and electrical properties will be significantly reduced. Most of the improvement technologies related to insulating paper only improve its hydrophobic properties. After damage, it is still irreparable or the repair effect is poor.
[0004] Patent CN114318942A discloses a method for preparing aminosilane-modified cellulose insulating paper for vegetable oil transformers, and the steps are as follows: the original insulating paper is transported to a cutting machine for cutting; the cut insulating paper is transported to a container for modification by soaking, wherein the container has three feeding ports, the first feeding port is opened to add a first volume of a solvent capable of dissolving 3-(aminopropyl)-triethoxysilane, and then the second feeding port is opened to add a second predetermined volume of 3-(aminopropyl)-triethoxysilane to obtain a colorless and transparent modified solution, at which time the insulating paper is fed in and the third feeding port is opened to add a third predetermined volume of n-butyl titanate as a catalyst, while uniform stirring is performed throughout the process to accelerate and maintain the homogenization of the solution; after soaking for a first predetermined time, the paper is sent out and passed through an ethanol cleaning area, and after washing off the residual liquid on the surface, it is continued to be sent to a first predetermined temperature drying area for drying for standby use.
[0005] Patent CN109024094A discloses a micro-nano cellulose fiber / aramid composite insulating paper and its preparation method. The composite insulating paper contains 30-70wt.% of aramid staple fibers, 20-50wt.% of aramid pulp and 10-20wt.% of micro-nano cellulose fibers. The aramid staple fibers, aramid pulp and micro-nano cellulose fibers are mixed with water, pulped and diluted to obtain slurry; the slurry is sent to a paper machine, formed into sheets, dried and hot-pressed to obtain micro-nano cellulose fiber / aramid composite insulating paper, the dielectric loss can reach 1.5-2, the cross-section quantitative unevenness is reduced to less than 3%, and the tensile strength and tear strength can be increased by more than 10%.
[0006] Patent CN113174783A discloses a method for preparing insulating paper with acid and alkali durability and hydrophobic self-repairing function. Insulating paperboard for transformers is used as the base material, and PTFE hydrophobic nanoparticles, fluorinated alkylsilane (FAS) and fluorocarbon surfactant ST-110 are the main raw materials. The three of them work together to form a dispersion that can be used as a coating in deionized water. NHCl4 is used as a suspending agent. After adding, the dispersion can form a durable and uniform coating solution in water. After the coating is evenly sprayed and dried, the insulating paper has good hydrophobic and oleophobic properties; it is durable and can be placed in air, water, and oil environments for more than 30 days without a significant decrease in performance; it has good acid and alkali resistance; at the same time, when the insulating paper can be wetted by water, it is not hydrophobic, but after heating at 130°C for 10 minutes, its hydrophobic properties can be restored.
[0007] However, the above-mentioned prior art still cannot solve the problems of poor hydrophobicity and lipophilicity of transformer insulation paper and insulation aging. The temperature of self-repair after physical damage is high, the energy consumption is still large, and the repair effect needs to be improved. Summary of the invention
[0008] The main purpose of the present invention is to provide a hydrophobic and oleophilic insulating paper, a preparation method and application thereof, so as to solve the problem that transformer insulating paper in the prior art cannot take into account good hydrophobicity and oleophilicity, insulation aging performance and self-repairing performance.
[0009] In order to achieve the above-mentioned object, according to one aspect of the present invention, there is provided a hydrophobic and oleophilic insulating paper, comprising a substrate paper, an organic coating and a carbon black coating, wherein the organic coating is located on both side surfaces of the substrate paper, and the carbon black coating is located on the surface of the organic coating away from the substrate paper; the organic coating comprises polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane.
[0010] Furthermore, the weight ratio of the organic coating to the substrate paper is (130-155):1; and / or the weight ratio of the carbon black coating to the substrate paper is (10-12):1.
[0011] Furthermore, the ratio of the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate to the weight of the substrate paper is (65-75):1; and / or the ratio of the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate to the volume of tridecafluorooctyl triethoxysilane is (65-75g):(50-55mL); and / or the weight ratio of polytetrafluoroethylene to perfluoroalkyl phosphate is 1:(2.5-3).
[0012] Furthermore, the contact angle of the hydrophobic and oleophilic insulating paper with water is 65 to 79°, and the contact angle with oil is 7 to 11°; and / or in the infrared spectrum of the hydrophobic and oleophilic insulating paper, at 1200 cm -1 and 1150cm -1 The CF stretching vibration peak appears at 800 cm -1 The Si-O absorption peak appears at 1710 cm -1 A CO bending peak and / or a C=O stretching vibration peak appear; and / or the hydrophobic and oleophilic insulating paper can self-repair after being physically damaged, and the self-repairing method is: drying the physically damaged hydrophobic and oleophilic insulating paper at 75-85° C. for 10-14 hours.
[0013] According to another aspect of the present invention, a method for preparing the hydrophobic and oleophilic insulating paper of the present invention is provided, comprising the following steps: step S1, mixing polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane, stirring to obtain an organic solution; step S2, immersing substrate paper in the organic solution, sequentially performing a first immersion and a first drying to obtain organic coated paper; step S3, immersing the organic coated paper in an ethanol dispersion of carbon black, sequentially performing a second immersion and a second drying to obtain hydrophobic and oleophilic insulating paper.
[0014] Further, step S1 comprises: mixing polytetrafluoroethylene and perfluoroalkyl phosphate, performing a first stirring to obtain a dispersion; then adding tridecafluorooctyl triethoxysilane to the dispersion, performing a second stirring to obtain an organic solution; preferably, the first stirring speed is 500 to 600 rpm, and the time is 25 to 35 min; and / or the second stirring speed is 300 to 400 rpm, and the time is 15 to 25 min.
[0015] Furthermore, in step S2, the first soaking time is 4 to 6 minutes; and / or the first drying includes a first drying step and a second drying step performed sequentially, the first drying step has a temperature of 20 to 30°C and a time of 8 to 12 minutes; the second drying step has a temperature of 30 to 40°C and a time of 25 to 35 minutes.
[0016] Furthermore, in step S3, the mass concentration of the ethanol dispersion of carbon black is 10 to 12 g / 100 mL; and / or the second immersion time is 4 to 6 min, the number of times is 3 to 4 times, and before each second immersion, the ethanol dispersion of carbon black is subjected to ultrasonic treatment for 4 to 6 min; and / or the carbon black is prepared by the following method: placing an aluminum foil above a lit candle, letting it stand, and scraping off the black substance on the aluminum foil to obtain carbon black.
[0017] According to another aspect of the present invention, an oil-paper insulation system is provided, comprising the hydrophobic and oleophilic insulation paper of the present invention.
[0018] According to another aspect of the present invention, a transformer is provided, comprising the above-mentioned oil-paper insulation system of the present invention.
[0019] By applying the technical solution of the present invention, by introducing polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane on the surface of substrate paper, and then introducing carbon black, the hydrophobic and oleophilic abilities of the insulating paper can be significantly improved, while at the same time enabling the paper to have damage self-repairing ability, and can also effectively delay the aging speed of the insulating paper under various stresses, so that the hydrophobic and oleophilic insulating paper can have good hydrophobic and oleophilic properties, insulation aging performance and self-repairing performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0021] Figure 1 The preparation flow chart according to Comparative Example 1 is shown;
[0022] Figure 2 The preparation flow chart of Example 1 according to the present invention is shown;
[0023] Figure 3 The scanning electron microscope images of the insulating paper according to the comparative example 1 and the embodiment 1 of the present invention are shown;
[0024] Figure 4 The infrared spectra of the insulating paper according to Comparative Example 1 and Example 1 of the present invention are shown;
[0025] Figure 5 The contact angle diagram of the insulating paper according to Comparative Example 1 and Example 1 of the present invention is shown;
[0026] Figure 6 The infrared spectra of the insulating paper before damage, after damage and after self-repair according to Example 1 of the present invention are shown;
[0027] Figure 7A graph showing the change in tensile strength of insulating paper according to Comparative Example 1 and Example 1 of the present invention with aging time is shown;
[0028] Figure 8 A graph showing the variation of the breakdown voltage of the insulating paper according to Comparative Example 1 and Example 1 of the present invention with the aging time is shown;
[0029] Fig. 9 The graphs showing the changes in dielectric constant and dielectric loss of insulating paper according to comparative example 1 and embodiment 1 of the present invention with aging time are shown.
[0030] The above drawings include the following reference numerals:
[0031] 1. Comparative Example 1; 2. Example 1; 3. Contact angle of Comparative Example 1 with water; 4. Contact angle of Example 1 with water; 5. Contact angle of Example 1 with oil. DETAILED DESCRIPTION
[0032] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0033] As described in the background of the present invention, there is a problem in the prior art that transformer insulation paper cannot take into account good hydrophobicity and oleophilicity, insulation aging performance and self-repairing performance. In order to solve the above problems, in a typical embodiment of the present invention, a hydrophobic and oleophilic insulation paper is provided, including substrate paper, an organic coating and a carbon black coating, the organic coating is located on the surface of both sides of the substrate paper, and the carbon black coating is located on the surface of the organic coating away from the substrate paper; the organic coating includes polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane. Among them, the substrate paper can use conventional types in the field, such as ordinary cellulose insulation paper.
[0034] The present invention forms an organic coating by introducing polytetrafluoroethylene (PTFE), perfluoroalkyl phosphate (FC-211) and tridecafluorooctyl triethoxysilane (POTS) on the surface of substrate paper, and a hydrophobic surface layer can be produced. Wherein PTFE can form a coating layer in the outer layer of the fiber structure of substrate paper, forming a surface with a better hydrophobic effect. Compared with other fluorocarbon surfactants, FC-211 is added less at the same dilution concentration, the pH value is neutral, and the stability is stronger at high temperatures, which is conducive to coordinating other components to improve the hydrophobicity and self-repairing properties of insulating paper, and can also reduce costs. Compared with other silanes, the surface free energy of POTS is lower, and it can be hydrolyzed and polycondensed with water in a humid environment to form a silicon dioxide base film and a self-repairing anti-corrosion polymer, and the hydrophobic self-repairing performance is better, and it has moderate hydrophobicity and oleophobicity, and other silanes generally have a relatively strong oleophobicity while being hydrophobic, and it is difficult to achieve a hydrophobic and lipophilic effect.
[0035] At the same time, carbon black is introduced on the surface of the organic coating to form a carbon black coating, which can increase the lipophilicity of the insulating paper surface. The oil contact angle of the carbon black particles is less than 20°, and the oil molecules (such as insulating oil) can enter the interior of the insulating paper faster through the carbon black particles, providing good lipophilicity without affecting the hydrophobic and electrical properties, and further increasing the oil immersion rate of the insulating paper, reducing the dielectric constant of the insulating paper, thereby improving the dielectric properties. The preferred carbon black mesh number is 180 to 220 meshes.
[0036] In summary, the insulating paper of the present invention utilizes organic coating to produce hydrophobic surface layer, and carbon black coating produces high oil adsorption, and both can form a coating layer in the outer layer of the fiber structure of substrate paper, forming an oleophilic and hydrophobic outer surface, playing a hydrophobic and oleophilic effect, so as to significantly improve the hydrophobic and oleophilic ability of insulating paper. At the same time, insulating paper can be made to have damage self-repairing ability, after physical damage, deep CF bond can be moved to coating surface by heat treatment, and the repair of Si-O-Si bond is promoted, so as to restore hydrophobic and oleophilic performance. In addition, the tensile strength and breakdown voltage of insulating paper are reduced with the decline of aging time, and dielectric constant and dielectric loss are reduced with the increase of aging time, so as to effectively delay the aging speed of insulating paper under various stresses. The insulating paper of the present invention has good hydrophobic and oleophilic performance, can effectively improve mechanical performance and electrical performance, solves the insulation aging problem in thermal aging process, and also has self-repairing ability after physical damage.
[0037] In a preferred embodiment, the weight ratio of the organic coating to the substrate paper is (130-155):1; and / or the weight ratio of the carbon black coating to the substrate paper is (10-12):1. Under the above conditions, the organic coating can be more fully wrapped around the outer layer of the fiber structure of the substrate paper to form a surface with better hydrophobicity, and the insulation aging performance and self-repairing performance of the insulating paper are further improved; the carbon black coating can be more evenly distributed on the surface of the organic coating, providing more excellent oleophilic properties, thereby better improving the hydrophobic and oleophilic abilities and dielectric properties of the insulating paper.
[0038] In order to further improve the hydrophobicity and self-healing properties of insulating paper and further slow down the aging rate of insulating paper under various stresses, in a preferred embodiment, the ratio of the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate to the weight of substrate paper is (65-75):1; and / or the ratio of the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate to the volume of tridecafluorooctyl triethoxysilane is (65-75g):(50-55mL); and / or the weight ratio of polytetrafluoroethylene to perfluoroalkyl phosphate is 1:(2.5-3).
[0039] As described above, the insulating paper of the present invention has good hydrophobic and oleophilic properties. In a preferred embodiment, the contact angle of the hydrophobic and oleophilic insulating paper with water is 65-79°, and the contact angle with oil is 7-11°; and / or in the infrared spectrum of the hydrophobic and oleophilic insulating paper, at 1200cm -1 and 1150cm -1 The CF stretching vibration peak appears at 800 cm -1 The Si-O absorption peak appears at 1710 cm -1 CO bending peaks and / or C=O stretching vibration peaks appear; and / or the hydrophobic and oleophilic insulating paper can self-repair after being physically damaged, and the self-repair method is: drying the physically damaged hydrophobic and oleophilic insulating paper at 75-85°C for 10-14h. Under the above conditions, the deep CF bonds can be more fully moved to the coating surface, and the repair of Si-O-Si bonds can be promoted, thereby restoring the hydrophobic and oleophilic properties more quickly.
[0040] In another typical embodiment of the present invention, a method for preparing the hydrophobic and oleophilic insulating paper of the present invention is also provided, comprising the following steps: step S1, mixing polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane, stirring to obtain an organic solution; step S2, immersing the substrate paper in the organic solution, sequentially performing a first immersion and a first drying to obtain an organic coated paper; step S3, immersing the organic coated paper in an ethanol dispersion of carbon black, sequentially performing a second immersion and a second drying to obtain a hydrophobic and oleophilic insulating paper.
[0041] The present invention first mixes polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane, stirs, and immerses the substrate paper in an organic solution, and performs a first immersion to form a hydrophobic organic coating on the surface of the substrate paper, and obtains an organic coating paper after a first drying; then the organic coating paper is immersed in an ethanol dispersion of carbon black, and a second immersion is performed to form an oleophilic carbon black coating on the surface of the organic coating, and ethanol can remove other substances remaining on the surface of the insulating paper or the organic coating, which plays a further cleaning role, and a hydrophobic and oleophilic insulating paper is obtained after a second drying. The above preparation method is simple, easy to operate, and is more conducive to preparing the insulating paper having good hydrophobic and oleophilic properties, insulation aging performance and self-repairing performance of the present invention.
[0042] In a preferred embodiment, step S1 includes: mixing polytetrafluoroethylene and perfluoroalkyl phosphate, performing a first stirring to obtain a dispersion; then adding tridecafluorooctyl triethoxysilane to the dispersion, performing a second stirring to obtain an organic solution; one of the main functions of POTS is to improve the difference in wettability and adsorption between PTFE and FC-211 due to the difference in properties, so first fully mixing PTFE and FC-211 and then adding POTS can better avoid the problem of particle agglomeration and further improve the conductivity and self-healing properties after coating. In order to achieve more complete mixing between the components of the organic coating, preferably, the speed of the first stirring is 500-600rpm, and the time is 25-35min; and / or the speed of the second stirring is 300-400rpm, and the time is 15-25min.
[0043] For the purpose of making the organic coating more fully coated on the surface of the substrate paper, in a preferred embodiment, in step S2, the first soaking time is 4 to 6 minutes; and / or the first drying includes a first drying step and a second drying step performed sequentially, the first drying temperature is 20 to 30° C., and the time is 8 to 12 minutes; the second drying temperature is 30 to 40° C., and the time is 25 to 35 minutes. Compared with the one-step drying treatment, the above two-step drying treatment can make the organic coating better coated on the surface of the substrate paper, further improving the coating completion.
[0044] In a preferred embodiment, in step S3, the mass concentration of the ethanol dispersion of carbon black is 10-12 g / 100 mL; and / or the second immersion time is 4-6 min, the number of times is 3-4 times, and the color change of the paper is observed to be obvious, and before each second immersion, the ethanol dispersion of carbon black is subjected to ultrasonic treatment for 4-6 min; and / or the carbon black is prepared by the following method: placing an aluminum foil above a lit candle, letting it stand, and scraping off the black substance on the aluminum foil to obtain carbon black. Under the above conditions, the carbon black coating can be more quickly and evenly applied to the surface of the organic coating to provide oleophilic properties, thereby further improving the oil immersion rate of the insulating paper, reducing the dielectric constant, and further improving the dielectric properties of the insulating paper.
[0045] In another typical embodiment of the present invention, an oil-paper insulation system is provided, comprising the hydrophobic and oleophilic insulation paper of the present invention. The insulating oil may be any conventional type in the art. Due to the use of the insulation paper of the present invention having good hydrophobic and oleophilic properties, insulation aging performance and self-repairing performance, the oil-paper insulation system can better maintain heat dissipation, insulation and arc extinguishing performance even under the influence of temperature and electromagnetic fields, and has excellent anti-aging performance.
[0046] In another typical embodiment of the present invention, a transformer is provided, including the oil-paper insulation system of the present invention, which can reduce the replacement frequency of insulation paper, thereby extending the service life of the transformer, which is beneficial to improving the voltage level of the power grid and maintaining safe and stable operation of the power grid.
[0047] Typically but not limiting, the weight ratio of the organic coating to the substrate paper is 130:1, 135:1, 140:1, 145:1, 150:1, 155:1 or a range consisting of any two of them; the weight ratio of the carbon black coating to the substrate paper is 10:1, 10.5:1, 11:1, 11.5:1, 12:1 or a range consisting of any two of them.
[0048] Typically, but not limiting, the ratio of the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate to the weight of the substrate paper is 65:1, 66:1, 67:1, 68:1, 69:1, 70:1, 71:1, 72:1, 73:1, 74:1, 75:1 or a range consisting of any two of them.
[0049] Typically but not limiting, when the total weight of polytetrafluoroethylene and perfluoroalkyl phosphate is 65g, 66g, 67g, 68g, 69g, 70g, 71g, 72g, 73g, 74g, 75g or a range consisting of any two of them, the volume of tridecafluorooctyl triethoxysilane is 50mL, 51mL, 52mL, 53mL, 54mL, 55mL or a range consisting of any two of them.
[0050] Typically but not limiting, the weight ratio of polytetrafluoroethylene to perfluoroalkyl phosphate is 1:2.5, 1:2.6, 1:2.7, 1:2.8, 1:2.9, 1:3 or a range consisting of any two of them.
[0051] A typical but non-limiting self-repairing method is: drying the physically damaged hydrophobic and oleophilic insulating paper at 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C or a range consisting of any two of their values for 10h, 11h, 12h, 13h, 14h or a range consisting of any two of their values.
[0052] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.
[0053] Comparative Example 1 Ordinary cellulose insulation paper (base paper)
[0054] Preparation flow chart see Figure 1 .
[0055] 1. Beating
[0056] (1) Cut wood pulp sheets into 2 cm × 2 cm pieces and soak them in deionized water for 20 hours to fully disintegrate;
[0057] (2) adding an appropriate amount of deionized water into a pulping machine according to the desired pulping concentration, starting the pulping machine, and adding the wood pulp sheets soaked in step (1);
[0058] (3) First, perform uniform mixing and beating for 5 minutes, then increase the pressure and evenly beat the pulp to 85° SR;
[0059] (4) After turning off the pulping machine, place the filter screen at the water outlet, open the valve to filter out the beaten pulp, first squeeze out most of the water in the pulp, and then place it on the filter screen and let it stand for a day to allow the excess water to be fully balanced;
[0060] (5) Place the pulp in a drying box for air drying to reduce its moisture content.
[0061] 2. Dissociation
[0062] In order to make the cellulose insulation paper prepared in the laboratory uniformly formed, with a smooth surface and uniform thickness, the pulp must first be subjected to a fiber dissociation process. The fiber dissociation operation allows the entangled cellulose in the pulp to be evenly distributed in deionized water without destroying its own structure, so that a uniform and flat surface can be formed in the subsequent paper forming process.
[0063] Dissociation step: After beating, put the prepared pulp into the dissociator, add deionized water to half the water level of the dissociator, set the speed of the dissociator to 12000, and dissociate 6 times. After each dissociation, let it stand for 1 minute before the next dissociation. After 6 dissociations, observe the dispersion of cellulose. Only when it meets the requirements can the next step be carried out. If the cellulose is not completely dispersed, the fiber dissociation operation should be carried out again.
[0064] 3. Molding
[0065] According to the conventional paper sheet forming method specified in the standard GB / T24324, the completely dissociated pulp is placed into the pulp storage chamber of the paper sheet forming machine, and appropriate water is added in proportion. Use vacuum filtration to form the prototype of insulating paper on the copper mesh, and use the supporting device to compact the insulating paper and remove excess water. Then use a shovel to shovel the paper off the copper mesh and put it into a vacuum dryer that has been preheated to 105°C. Put a copper mesh on its surface to prevent it from adhering to the cover of the dryer. Turn on the vacuum pump, exhaust the air, and dry it for 5 minutes under the conditions of 92Pa vacuum and 105°C. In order to prevent the dried paper from being contaminated by moisture in the vacuum pump, the vacuum valve should be closed first and then the vacuum pump should be turned off. Finally, the vacuum dryer is turned on to obtain the ordinary cellulose insulating paper (substrate paper) prepared in the laboratory.
[0066] Example 1
[0067] Preparation flow chart see Figure 2 .
[0068] 1. Preparation of organic solution
[0069] (1) Weighing 72 g of polytetrafluoroethylene (PTFE) and perfluoroalkyl phosphate (FC-211) in a mass ratio of 1:2.8, fully mixing and dispersing them, and stirring them on a magnetic stirrer at 550 rpm for 30 min until a uniform dispersion is formed;
[0070] (2) Add 52 ml of tridecafluorooctyl triethoxysilane (POTS) to the above dispersion, stir at 350 rpm for 20 min on a magnetic stirrer after it is fully dissolved to obtain a uniform solution without solid powder. Let it stand for 1 hour to obtain the desired organic solution. Check that there is no precipitate and store it for future use.
[0071] 2. Carbon black preparation
[0072] Place aluminum foil above a lit candle and judge the amount of carbon black by the darkness of the foil. Then scrape the carbon black on the foil into a beaker for later use. The foil can be used repeatedly. After the carbon black is dried, take 11 g and add 100 mL of ethanol for 5 minutes of ultrasonic dispersion to obtain a carbon black ethanol dispersion with a mass concentration of 11 g / 100 mL.
[0073] 3. Coating process
[0074] 1 g of the ordinary cellulose insulation paper of Comparative Example 1 was immersed in the organic solution for 5 minutes, then dried at 25° C. for 10 minutes, and finally placed in a drying oven at 35° C. for 30 minutes before being taken out to obtain an organic coated paper;
[0075] The organic coated paper was immersed in 100 mL of carbon black ethanol dispersion for 5 minutes and dried. The amount of carbon black on the surface of the organic coated paper was increased by repeating the immersion-drying process 4 times. The carbon black ethanol dispersion was ultrasonically treated for 5 minutes before each immersion to ensure that the carbon black could be evenly attached to the surface of the organic coated paper to obtain hydrophobic and oleophilic insulating paper.
[0076] Performance Test:
[0077] In order to observe the microscopic changes of the novel hydrophobic and oleophilic insulating paper, the microscopic morphology of the insulating paper of Comparative Example 1 and Example 1 was observed using a scanning electron microscope (see the scanning electron microscope image). Figure 3 , where 1 is comparative example 1 and 2 is embodiment 1). By comparison, it can be found that the surface of the ordinary cellulose insulation paper of comparative example 1 is smooth and flat, while the surface of the new hydrophobic and oleophilic insulation paper after coating treatment in embodiment 1 is uneven, and a layer of carbon black particles and PTFE nanoparticles are coated on the surface, which is equivalent to forming a coating layer on the outer layer of the fiber structure, playing a hydrophobic role.
[0078] In order to verify whether the coating of the insulating paper is complete, the insulating paper before and after coating (Comparative Example 1 is before coating, Example 1 is after coating) was compared by Fourier transform infrared spectroscopy (infrared spectrum see Figure 4 , where 1 is comparative example 1 and 2 is example 1). The insulating paper of example 1 is -1 and 1150cm -1 A new peak appears, which is indicative of CF stretching vibration; 800 cm -1 The peak is the Si-O absorption of fluorinated alkylsilane; 1710 cm -1 The peaks of correspond to the CO bending and C=O stretching vibrations of FC-211 and carbon black particles. This proves the successful coating of the coating in Example 1.
[0079] In order to verify the hydrophobicity and lipophilicity of the insulating paper, the contact angle was tested and compared (see the contact angle diagram Figure 5 , where 3 is the contact angle of comparative example 1 with water, 4 is the contact angle of embodiment 1 with water, and 5 is the contact angle of embodiment 1 with oil). The contact angle of the insulating paper of comparative example 1 without coating with water is 43°, while the contact angle of the insulating paper of embodiment 1 after coating with water is increased to 79°, and the contact angle with oil is 7°, which proves that the new hydrophobic and oleophilic insulating paper of embodiment 1 has good hydrophobic and oleophilic properties.
[0080] In order to verify the self-repairing ability of the insulating paper after physical damage, the surface of the new hydrophobic and oleophilic insulating paper of Example 1 was scratched with abrasive paper to reduce its hydrophobicity, and then the coated insulating paper after physical damage was placed in an oven at 80°C for 12 hours of heat treatment. The infrared spectra before and after damage and after self-repair were compared (the infrared spectra of the insulating paper before damage, after damage and after self-repair are shown in Figure 6 ).
[0081] Before damage, the new hydrophobic and oleophilic insulating paper is -1 and 1150cm -1 A new peak appears near 800 cm, which is due to the CF stretching vibration; -1 The peak is the Si-O absorption of tridecafluorooctyltriethoxysilane; 1710cm -1 The peaks correspond to the CO bending and C=O stretching vibrations of FC-211 and carbon black particles. This indicates the presence of a coating.
[0082] After damage, the new hydrophobic and oleophilic insulating paper has a -1 、1200cm -1 and 1150cm -1 The peak at 800cm -1 This indicates that when the surface of the new hydrophobic and oleophilic insulating paper is worn, the CF bonds and Si-O bonds are removed from the coating surface, and other functional groups are also damaged.
[0083] After repair, when the damaged new hydrophobic and oleophilic insulating paper was heated, the CF bonds reappeared and the CF peak was significantly enhanced (absorbance changed from 0.0524 to 0.1067), indicating that the heat treatment caused the CF chains to move to the coating surface. -1 The characteristic peak nearby also slightly enhances (the absorbance changes from 0.0253 to 0.0503), indicating that heating also has a certain enhancing effect on the repair of Si-O-Si bonds.
[0084] In order to determine the thermal aging performance of the novel hydrophobic and oleophilic insulating paper of Example 1 in actual use, a 45-day artificial simulated thermal aging test was carried out on it according to standard IEC 62332-2:2014, and the mechanical and electrical properties of the paper at different stages of the aging process were tested.
[0085] The variation of the tensile strength of the insulating paper of Comparative Example 1 and Example 1 with the aging time is shown in Figure 7, where 1 is Comparative Example 1, and 2 is Example 1. It can be observed that in the first 2 days of accelerated thermal aging, the tensile strength of the insulating paper of Comparative Example 1 and Example 1 increases within a small range. This is because the first 2 days are equivalent to the annealing stage in industrial production, which releases a small amount of internal stress of cellulose, and thus the tensile strength of the insulating paper increases. With the deepening of aging, the tensile strength of both insulating papers shows a significant downward trend, and the decline is relatively fast in the early stage of aging, and the decline rate gradually tends to be flat in the later stage of aging. Moreover, during the aging process, the tensile strength of the insulating paper of Example 1 always remains higher than that of Comparative Example 1. After the aging process, the tensile strength of the insulating paper of Example 1 is increased by 11.6% compared with that of Comparative Example 1.
[0086] The variation of the breakdown voltage of the insulating paper of Comparative Example 1 and Example 1 with the aging time is shown in FIG. Figure 8 , where 1 is comparative example 1 and 2 is example 1. It can be observed that with the increase of aging time, the breakdown voltage of both insulating papers shows a downward trend as a whole, and the insulating paper of example 1 is always higher than the insulating paper of comparative example 1. After aging, the breakdown voltage of the insulating paper of example 1 is increased by 4.84% compared with that of comparative example 1. This is because the insulating paper modified by the coating in example 1 can maintain a high breakdown field strength for a long time without causing a significant decrease in the breakdown voltage due to aging, because the dielectric constant of the new hydrophobic and oleophilic insulating paper is smaller than that of the ordinary cellulose insulating paper in comparative example 1, and is closer to the dielectric constant of the insulating oil, and therefore has a higher short-term AC breakdown strength during the aging process.
[0087] The change of dielectric constant and dielectric loss of insulating paper of comparative example 1 and embodiment 1 with aging time is shown in Fig. 9, where 1 is comparative example 1 and 2 is example 1. It can be observed that with the increase of aging time, these two parameters of the two insulating papers show an increasing trend, and the insulating paper after coating modification in example 1 is always smaller than the unmodified insulating paper in comparative example 1. The reason is that the aging of the insulating paper will produce more polar substances, resulting in an increase in the relative dielectric constant. During the entire aging process, the relative dielectric constant of the new hydrophobic and oleophilic insulating paper modified by coating in example 1 is lower than that of the ordinary cellulose insulating paper in comparative example 1. This is because the relative dielectric constant of the coating material is small, and the introduction of the coating reduces the overall dielectric constant of the insulating paper. In addition, the apparent free energy of the coating is very low and most of it is organic matter, which makes it difficult to decompose polar substances during the aging process, so that the coating has good stability. As aging proceeds, the new hydrophobic and oleophilic insulating paper in example 1 has better thermal stability and can delay the aging of the insulating paper, so its relative dielectric constant and dielectric loss factor are smaller than those of the ordinary cellulose insulating paper in comparative example 1. Compared with comparative example 1, the relative dielectric constant and dielectric loss factor of the insulating paper in Example 1 are reduced by 10.02% and 11.26%, respectively. Therefore, the addition of the coating can increase the dielectric properties of the insulating paper and slow down its aging rate.
[0088] Example 2
[0089] The difference from Example 1 is that during the preparation of the organic solution:
[0090] (1) Weighing 65 g of polytetrafluoroethylene (PTFE) and perfluoroalkyl phosphate (FC-211) in a mass ratio of 1:2.5, fully mixing and dispersing them, and stirring them on a magnetic stirrer at 500 rpm for 35 min until a uniform dispersion is formed;
[0091] (2) Add 50 ml of tridecafluorooctyl triethoxysilane (POTS) to the above dispersion, stir at 300 rpm for 25 min on a magnetic stirrer after it is fully dissolved to obtain a uniform solution without solid powder. Let it stand for 1 hour to obtain the desired organic solution. Check that there is no precipitate and store it for future use.
[0092] Example 3
[0093] The difference from Example 1 is that during the preparation of the organic solution:
[0094] (1) Weighing 75 g of polytetrafluoroethylene (PTFE) and perfluoroalkyl phosphate (FC-211) in a mass ratio of 1:3, fully mixing and dispersing them, and stirring them on a magnetic stirrer at 600 rpm for 25 min until a uniform dispersion is formed;
[0095] (2) Add 55 ml of tridecafluorooctyl triethoxysilane (POTS) to the above dispersion, stir at 400 rpm for 15 min on a magnetic stirrer after it is fully dissolved to obtain a uniform solution without solid powder. Let it stand for 1 hour to obtain the desired organic solution. Check that there is no precipitate and store it for future use.
[0096] Example 4
[0097] The difference from Example 1 is that in the preparation of carbon black,
[0098] Place aluminum foil above a lit candle and judge the amount of carbon black by the darkness of the foil. Then scrape the carbon black on the foil into a beaker for later use. The foil can be used repeatedly. After the carbon black is dried, take 10g and add 100mL of ethanol for 5 minutes of ultrasonic dispersion to obtain a carbon black ethanol dispersion with a mass concentration of 10g / 100mL.
[0099] Example 5
[0100] The difference from Example 1 is that in the preparation of carbon black,
[0101] Place aluminum foil above a lit candle and judge the amount of carbon black by the darkness of the foil. Then scrape the carbon black on the foil into a beaker for later use. The foil can be used repeatedly. After the carbon black is dried, take 12 g and add 100 mL of ethanol for 5 minutes of ultrasonic dispersion to obtain a carbon black ethanol dispersion with a mass concentration of 12 g / 100 mL.
[0102] Example 6
[0103] The difference from Example 1 is that during the coating process,
[0104] 1 g of the common cellulose insulating paper of Comparative Example 1 was immersed in the organic solution for 4 minutes, then dried at 20° C. for 8 minutes, and finally dried in a drying oven at 30° C. for 35 minutes before being taken out to obtain an organic coated paper.
[0105] Example 7
[0106] The difference from Example 1 is that during the coating process,
[0107] 1 g of the common cellulose insulating paper of Comparative Example 1 was immersed in the organic solution for 6 minutes, then dried at 30° C. for 12 minutes, and finally dried in a drying oven at 40° C. for 25 minutes before being taken out to obtain an organic coated paper.
[0108] Example 8
[0109] The difference from Example 1 is that during the coating process,
[0110] The organic coated paper was immersed in 100 mL of carbon black ethanol dispersion for 4 minutes and dried. The amount of carbon black on the surface of the organic coated paper was increased by repeating the immersion-drying process 3 times. The carbon black ethanol dispersion was ultrasonically treated for 4 minutes before each immersion to ensure that the carbon black could be evenly attached to the surface of the organic coated paper to obtain hydrophobic and oleophilic insulating paper.
[0111] Example 9
[0112] The difference from Example 1 is that during the coating process,
[0113] The organic coated paper was immersed in 100 mL of carbon black ethanol dispersion for 6 minutes and dried. The amount of carbon black on the surface of the organic coated paper was increased by repeating the immersion-drying process 4 times. The carbon black ethanol dispersion was ultrasonically treated for 6 minutes before each immersion to ensure that the carbon black could be evenly attached to the surface of the organic coated paper to obtain hydrophobic and oleophilic insulating paper.
[0114] Example 10
[0115] The difference from Example 1 is that, in the process of verifying the self-repairing ability of the insulating paper after physical damage, the surface of the new hydrophobic and oleophilic insulating paper of Example 1 is scratched with sandpaper to reduce its hydrophobicity, and then the coated insulating paper after physical damage is placed in an oven at 75°C for heat treatment for 14 hours.
[0116] Embodiment 11
[0117] The difference from Example 1 is that, in the process of verifying the self-repairing ability of the insulating paper after physical damage, the surface of the new hydrophobic and oleophilic insulating paper of Example 1 is scratched with sandpaper to reduce its hydrophobicity, and then the coated insulating paper after physical damage is placed in an oven at 85°C for heat treatment for 10 hours.
[0118] Comparative Example 2
[0119] The difference from Example 1 is that the fluorocarbon surfactant used in the organic solution is ST-110.
[0120] The test results of the insulation paper properties of the above embodiments and comparative examples are shown in Table 1.
[0121] Among them, the damage self-repair performance is judged by the peak changes of CF bond and Si-O bond in the infrared spectrum before and after damage self-repair. If the two peaks remain unchanged after self-repair, it is recorded as "none", if the increase of both peaks is less than 0.01, it is recorded as "poor", if the increase of both peaks is greater than 0.01 and less than 1.8 times of the peak before repair, it is recorded as "medium", and if the increase of both peaks is greater than 1.8 times of the peak before repair, it is recorded as "excellent".
[0122] Test method:
[0123] Contact angle: BX53M optical microscope, magnification ×800;
[0124] Tensile strength: XLW (PC) intelligent electronic tensile testing machine;
[0125] Breakdown voltage: Standard IEC 60243-1:2013;
[0126] Dielectric constant: Concept 80 broadband dielectric constant meter;
[0127] Dielectric loss: Concept 80 broadband dielectric meter.
[0128] Table 1
[0129]
[0130] As can be seen from the above, compared with the comparative example, the embodiments of the present invention can significantly improve the hydrophobic and oleophilic ability of the insulating paper by introducing polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane on the surface of the substrate paper, and then introducing carbon black, while making it have both damage self-repair ability, and can also effectively delay the aging speed of the insulating paper under various stresses, so that the hydrophobic and oleophilic insulating paper can take into account good hydrophobic and oleophilic properties, insulation aging performance and self-repair performance. In addition, it can be seen that when the process parameters are within the preferred range of the present invention, the comprehensive performance of the insulating paper is better.
[0131] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A hydrophobic and oleophilic insulating paper, characterized in that: It comprises a substrate paper, an organic coating and a carbon black coating, wherein the organic coating is located on both sides of the substrate paper, and the carbon black coating is located on the surface of the organic coating away from the substrate paper; The organic coating comprises polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane.
2. The hydrophobic and oleophilic insulating paper according to claim 1, characterized in that: The weight ratio of the organic coating to the substrate paper is (130-155):1; and / or The weight ratio of the carbon black coating to the substrate paper is (10-12):
1.
3. The hydrophobic and oleophilic insulating paper according to claim 1 or 2, characterized in that: The ratio of the total weight of the polytetrafluoroethylene and the perfluoroalkyl phosphate to the weight of the substrate paper is (65-75):1; and / or The ratio of the total weight of the polytetrafluoroethylene and the perfluoroalkyl phosphate to the volume of the tridecafluorooctyl triethoxysilane is (65-75 g): (50-55 mL); and / or The weight ratio of the polytetrafluoroethylene to the perfluoroalkyl phosphate is 1:(2.5-3).
4. The hydrophobic and oleophilic insulating paper according to any one of claims 1 to 3, characterized in that: The contact angle of the hydrophobic and oleophilic insulating paper with water is 65-79°, and the contact angle with oil is 7-11°; and / or In the infrared spectrum of the hydrophobic and oleophilic insulating paper, at 1200 cm -1 and 1150cm -1 The CF stretching vibration peak appears at 800 cm -1 The Si-O absorption peak appears at 1710 cm -1 The presence of CO bending peaks and / or C=O stretching vibration peaks; and / or The hydrophobic and oleophilic insulating paper can self-repair after being physically damaged, and the self-repairing method is: drying the physically damaged hydrophobic and oleophilic insulating paper at 75-85° C. for 10-14 hours.
5. The method for preparing the hydrophobic and oleophilic insulating paper according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step S1, mixing polytetrafluoroethylene, perfluoroalkyl phosphate and tridecafluorooctyl triethoxysilane, and stirring to obtain an organic solution; Step S2, immersing the substrate paper in the organic solution, and sequentially performing a first immersion and a first drying to obtain an organic coated paper; Step S3, immersing the organic coated paper in an ethanol dispersion of carbon black, and sequentially performing a second immersion and a second drying to obtain the hydrophobic and oleophilic insulating paper.
6. The preparation method according to claim 5, characterized in that: The step S1 comprises: The polytetrafluoroethylene and the perfluoroalkyl phosphate are mixed and first stirred to obtain a dispersion; then the tridecafluorooctyl triethoxysilane is added to the dispersion and second stirred to obtain the organic solution; Wherein, the rotation speed of the first stirring is 500-600 rpm, and the time is 25-35 min; and / or the rotation speed of the second stirring is 300-400 rpm, and the time is 15-25 min.
7. The preparation method according to claim 5 or 6, characterized in that: In the step S2, The first soaking time is 4 to 6 minutes; and / or The first drying comprises a first drying step and a second drying step which are performed sequentially, wherein the first drying step is performed at a temperature of 20 to 30° C. and lasts for 8 to 12 minutes; and the second drying step is performed at a temperature of 30 to 40° C. and lasts for 25 to 35 minutes.
8. The preparation method according to any one of claims 5 to 7, characterized in that: In the step S3, the mass concentration of the carbon black ethanol dispersion is 10-12 g / 100 mL; and / or The second immersion time is 4 to 6 minutes, the number of times is 3 to 4 times, and before each second immersion, the carbon black ethanol dispersion is subjected to ultrasonic treatment for 4 to 6 minutes; and / or The carbon black is prepared by the following method: placing an aluminum foil above a lit candle, leaving it to stand, and scraping off the black material on the aluminum foil to obtain the carbon black.
9. An oil-paper insulation system, characterized in that: The invention comprises the hydrophobic and oleophilic insulating paper according to any one of claims 1 to 4.
10. A transformer, characterized in that: Comprising the oil-paper insulation system as claimed in claim 9.
Citation Information
Patent Citations
High-conductivity aramid insulation paper-based material for large oil-immersed transformer and preparation method of high-conductivity aramid insulation paper-based material
CN112681010A
Preparation method of insulating paper with acid-base durability and hydrophobic self-repairing function
CN113174783A
Insulated wire for oil-immersed transformer
JP1995320546A
Electrical insulating paper and stationary induction electrical device therewith
JP2016204760A