Method for detecting foreign matters wrapped in PE powder
Through magnetic rod adsorption and heating extraction technology, combined with elemental analysis, it solves the problem that existing technology cannot detect foreign matter in PE powder, achieves rapid and accurate detection of foreign matter in lithium battery separators, and improves the quality and safety of the separator.
Patent Information
- Application Number
- CN202411147620.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-10-08
AI Technical Summary
Existing technology cannot effectively detect magnetic or non-magnetic foreign matter wrapped in PE powder, which affects the quality and safety of lithium battery separators.
After using a magnetic rod to absorb the PE powder, dissolve it in the solvent to form a mixture and heat it to a molten state. Observe whether there is any insoluble matter, then extract and grind it, and detect the presence and composition of the insoluble matter through qualitative analysis of elemental components.
It achieves fast and accurate detection of foreign matter wrapped in PE powder, can detect magnetic and non-magnetic foreign matter, and improves the quality control capability of lithium battery separators.
Abstract
Description
Technical Field
[0001] The invention relates to an industrial detection method, in particular to a method for detecting foreign matter in the production of lithium battery separators, and specifically to a method for detecting foreign matter wrapped in PE powder. Background Art
[0002] The main function of lithium battery separators is to separate the positive and negative electrodes of the battery to prevent the two electrodes from contacting and short-circuiting. The performance of the separator determines the interface structure and internal resistance of the battery, which directly affects the battery's capacity, cycle and safety performance. A separator with excellent performance plays an important role in improving the overall performance of the battery. Foreign matter in the separator directly affects the safety of the battery. Therefore, major car manufacturers and battery manufacturers pay special attention to the control of foreign matter in the separator. The source of foreign matter in the separator is mainly introduced by the raw material PE (polyethylene) powder. Therefore, the control of foreign matter in PE powder is particularly important.
[0003] At present, the method for detecting magnetic substances in PE powder is: stir the PE powder with a magnetic bar to extract the magnetic substances, and the powder with magnetic substances on the surface is adsorbed on the magnetic bar, and then the powder is analyzed and detected by the automatic cleanliness analysis system to determine the size and quantity of the magnetic substances. However, this method can only detect the adsorption of magnetic substances on the outside of PE powder, and cannot detect magnetic or non-magnetic substances that may be wrapped in PE powder, which will have a great impact on the quality of subsequent diaphragms.
[0004] Therefore, it is urgent to design a detection method so that foreign matter in PE powder can be detected conveniently and quickly. Summary of the invention
[0005] The purpose of the present invention is to provide a method for detecting foreign matter wrapped in PE powder in response to the problems currently existing in the detection process of PE powder, a raw material for diaphragm production, which can conveniently and quickly detect non-magnetic foreign matter wrapped in PE powder and perform qualitative analysis, thereby creating favorable conditions for improving the quality of lithium battery diaphragm products.
[0006] The technical solution of the present invention is: A method for detecting foreign matter contained in PE powder comprises the following steps: 1) Adsorb the PE powder to be tested on a magnetic rod; 2) dissolving the PE powder adsorbed in step 1) in a solvent to form a mixture; 3) Take out an appropriate amount of the mixture, clamp it between two slides, and heat the slides to a set temperature to melt the PE powder; while heating, observe whether there is insoluble matter in the mixture in the slides; if there is insoluble matter, go to the next step; if there is no insoluble matter, the detection operation is completed; 4) Cooling the slide to room temperature so that the molten material held therein forms a solid sample to be tested; then, removing the slide, and placing the sample to be tested in an extractant for extraction; 5) taking out the sample to be tested from the extractant, drying it and then grinding it to expose the cross section of the insoluble matter therein; 6) Conduct qualitative analysis of the elemental composition of the cross section of the insoluble matter.
[0007] Furthermore, in the step 1), the PE powder to be tested is placed in anhydrous ethanol and stirred using a magnetic bar, and then the solution is filtered and the filtrate is dried.
[0008] Furthermore, in the step 1), the stirring time using the magnetic bar is 5 min to 20 min.
[0009] Furthermore, in the step 1), the drying temperature is 70° C.-90° C., optionally 80° C.; the drying time is 0.5 h-2 h, optionally 1 h.
[0010] Furthermore, the solvent is mineral oil; preferably, the mineral oil is paraffin oil or white oil; the ratio of the PE powder to the solvent is: (0.5:1)-(4:1).
[0011] Furthermore, in step 3), the mixture is dropped onto a slide using a pipette, and then another slide is pressed on top, so that a closed space with a certain internal pressure is formed between the two slides.
[0012] Furthermore, in the step 3), the slide is placed on a heating fixture of a hot stage for heating and is observed through a microscope on the hot stage. The heating device may also be an oven or a muffle furnace.
[0013] Furthermore, in step 3), the microscope is an optical microscope, for example, an ordinary microscope, and can further be an ordinary microscope used in conjunction with a hot stage.
[0014] Furthermore, in the step 3), the heating stage is heated at a maximum heating rate.
[0015] Furthermore, in the step 3), the slide is heated to 130°C to 220°C.
[0016] Furthermore, in the step 3), whether insoluble matter can be observed in the mixture under a microscope with a magnification of 20X is generally used as a basis for determining whether to continue the detection method.
[0017] Furthermore, in step 4), the extractant is dichloromethane, methanol or ethyl acetate; preferably, the extractant is dichloromethane; the mass ratio of the dichloromethane to the solvent added in step 2 is (48:1)-(52:1).
[0018] Furthermore, in step 5), the sample to be tested needs to be ground under a microscope; preferably, the microscope can be roughly adjusted first to find the sample, and then finely adjusted, and ground on the basis that the sample is clearly displayed in the field of view, and the magnification of the microscope includes but is not limited to 5X, 10X, 20X, 30X, 40X or 50X.
[0019] Furthermore, in step 5), the microscope may be an optical microscope, for example, an ordinary microscope.
[0020] Furthermore, the qualitative analysis of elemental composition in step 6) may be performed using EDS or XPS.
[0021] Beneficial effects of the present invention: The invention has reasonable design and convenient operation, can quickly and accurately detect magnetic and non-magnetic foreign matter wrapped in PE powder, and can perform qualitative analysis on the detected foreign matter, thus creating favorable conditions for quality control of subsequent diaphragm production. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with the embodiments. Embodiment 1
[0023] A method for detecting foreign matter contained in PE powder comprises the following steps: 1) 300g PE powder is placed in a 2000ml beaker, and then 800ml anhydrous ethanol is added to form a uniformly mixed suspension; then, a magnetic bar is used to uniformly stir for about 10 minutes so that the magnetic bar can fully absorb the magnetic substance in the solution; then, the solution is filtered and the filtrate is dried; the drying temperature is about 80°C and the drying time is about 1h; 2) taking 0.5 g of the PE powder dried in step 1) and 1 g of white oil and mixing them to form a uniform mixture; 3) Use a pipette to drop 1 drop of the mixture in step 2) onto a slide, and press another slide on top of it to form a closed space with a certain internal pressure between the two slides, so as to be more conducive to the dissolution and mixing of PE powder; then, place the slide on the hot stage heating fixture in a common microscope connected to a hot stage, and heat the hot stage to 180°C at the maximum heating rate to fully melt the PE powder; at the same time, observe whether there is insoluble matter in the mixture in the slide through the microscope on the hot stage; if there is insoluble matter, go to the next step; if there is still no insoluble matter under the condition of a magnification of 20X, it is determined that there is no foreign matter, and this detection operation is completed; 4) Cooling the slide to room temperature to form a solid sheet of the sample to be tested in the molten material held therein; then, removing the slide, placing the sample to be tested in 50 g of dichloromethane solution for extraction to remove the white oil therein; 5) taking out the sample to be tested from the dichloromethane solution, drying it to remove the dichloromethane, and then grinding it under a common microscope (the insoluble matter can be focused at a magnification of 5X, and then the magnification can be increased in sequence based on the different sizes of the insoluble matter particles, so that the target object can be clearly seen) to expose the cross section of the insoluble matter; 6) Perform EDS (Energy Dispersive Spectroscopy) qualitative analysis on the cross section of the insoluble matter to provide a basis for the subsequent treatment of the raw PE powder.
[0024] In the present application, the insoluble matter refers to granular solids with a particle size ranging from 20 um to 400 um in the PE slurry formed into a molten state by heating.
[0025] Among them, the ordinary microscope is a Jiangnan Yongxin MV3000 equipped with a hot stage controlled by an Instec mk2000 temperature control system. Embodiment 2
[0026] The operation steps of the second embodiment are basically the same as those of the first embodiment, with the main difference being: 1. In step 2), 4 g of dried PE powder and 1 g of white oil are mixed to form a mixture; 2. In step 3), heat the hot plate at the maximum rate to 200°C.
[0027] In both of the above two embodiments, the PE powder samples can be melted quickly and completely, and the presence of insoluble matter within the field of view can be directly observed through a microscope. At the same time, it can also be concluded from the above embodiments that: 1) As the ratio of PE powder to white oil increases, the difficulty of melting PE powder will increase. At the same time, if the ratio of PE powder to white oil is too low, there will be too few PE particles in the microscope field of view, which is not conducive to observation.
[0028] 2) Within the range of the heating temperature of the hot plate, the higher the heating temperature, the faster the PE powder melts. However, if it exceeds 220°C, the PE powder will decompose and affect the detection effect; if it is lower than 130°C, the PE powder will not be completely melted, affecting the detection effect.
[0029] The present invention can quickly and accurately detect magnetic and non-magnetic foreign matter wrapped in PE powder, and can perform qualitative analysis on the detected foreign matter, thus creating favorable conditions for quality control of subsequent diaphragm production.
[0030] The parts not involved in the present invention are the same as the prior art or can be implemented by using the prior art.
Claims
1. A method for detecting foreign matter contained in PE powder, characterized in that: The following steps are involved: 1) Adsorb the PE powder to be tested on a magnetic rod; 2) dissolving the PE powder adsorbed in step 1) in a solvent to form a mixture; 3) Take out an appropriate amount of the mixture, clamp it between two slides, and heat the slides to a set temperature to melt the PE powder; while heating, observe whether there is insoluble matter in the mixture in the slides; if there is insoluble matter, go to the next step; if there is no insoluble matter, the detection operation is completed; 4) Cooling the slide to room temperature so that the molten material held therein forms a solid sample to be tested; then, removing the slide, and placing the sample to be tested in an extractant for extraction; 5) taking out the sample to be tested from the extractant, drying it and then grinding it to expose the cross section of the insoluble matter therein; 6) Conduct qualitative analysis of the elemental composition of the cross section of the insoluble matter.
2. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 1), the PE powder to be tested is placed in anhydrous ethanol and stirred with a magnetic bar. Then, the solution is filtered and the filtered product is dried.
3. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 1), the stirring time using the magnetic bar is 5 min to 20 min.
4. The method for detecting foreign matter contained in PE powder according to claim 2, characterized in that: The drying temperature is 70℃-90℃, and the drying time is 0.5h-2h.
5. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 2), the solvent is mineral oil; preferably, the mineral oil is paraffin oil or white oil; the ratio of the PE powder to the solvent is: (0.5:1)-(4:1).
6. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 3), the mixture is dropped onto a slide using a pipette, and then another slide is pressed on top to form a closed space with a certain internal pressure between the two slides.
7. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 3), the slide is placed on a heating fixture of a hot stage for heating, and is observed through a microscope on the hot stage; preferably, the hot stage is heated at a maximum heating rate; preferably, the slide is heated to 130° C. to 220° C.
8. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 4), the extractant is dichloromethane, methanol or ethyl acetate; preferably, the extractant is dichloromethane; the mass ratio of the dichloromethane to the solvent added in the step 2 is (48:1)-(52:1).
9. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In the step 5), the sample to be tested needs to be ground under a microscope.
10. The method for detecting foreign matter contained in PE powder according to claim 1, characterized in that: In step 6), the element composition is qualitatively analyzed using EDS or XPS.