Negative electrode coating, negative electrode and lithium ion battery

By improving the composition of the negative electrode coating and the coordination of the electrolyte, the problems of poor electrolyte wettability and increased interface impedance caused by the inorganic ceramic negative electrode coating are solved, improving the safety performance and consistency of lithium-ion batteries and reducing production costs. energy consumption.

CN118748239APending Publication Date: 2024-10-08SHANGHAI TAIRUI LITHIUM BATTERY TECHNOLOGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411116588.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The introduction of inorganic ceramic negative electrode coatings in existing lithium-ion batteries has resulted in poor electrolyte wettability, prolonged standing time, increased interface impedance, and lithium precipitation problems. In addition, water absorption by nanoparticles during the production process increases production energy consumption and affects battery consistency. sex.

Method used

Using a negative electrode coating composed of binders, inorganic ceramics, organic solvents and additives, by improving the hydrophobicity, lipophilicity and solid content of the coating, combined with high wettability electrolyte, the interface resistance and water absorption are reduced, and the wetting of the electrolyte is improved. and retention.

Benefits of technology

It alleviates the impact of water absorption of the negative electrode coating on battery consistency, reduces production energy consumption, improves safety performance and cycle life, reduces lithium deposition problems, and improves battery safety performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748239A_ABST
    Figure CN118748239A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of lithium batteries, in particular to a negative electrode coating, a negative electrode and a lithium ion battery. The negative electrode coating is formed by curing coating slurry, the coating slurry comprises a binder, inorganic ceramic, a first organic solvent and an additive, and the additive comprises at least one of fluorinated polyethylene, expanded graphite and fluorocarbon wax. According to the technical scheme, the negative electrode coating is improved, the influence of water absorption of the negative electrode coating on the consistency of the battery is relieved, the production energy consumption is reduced, the production efficiency is improved, the interface impedance is reduced, the generation of lithium dendrites is inhibited, the lithium precipitation problem is relieved, and the safety performance is improved; and moreover, the negative electrode coating is matched with the high-wettability electrolyte, so that the water absorption of the negative electrode is reduced, the wetting and retaining force of the negative electrode to the electrolyte is greatly improved, the battery polarization is reduced, and the safety performance is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium batteries, and in particular to a negative electrode coating, a negative electrode and a lithium ion battery. Background Art

[0002] As the application fields of lithium-ion batteries continue to expand, more and more attention is paid to the energy density and safety performance of lithium-ion batteries. In order to improve the safety performance of high-energy-density battery systems, related technologies often coat inorganic ceramic negative electrode coatings on the electrode surface to improve thermal and mechanical safety performance.

[0003] However, the introduction of inorganic ceramic negative electrode coating will cause the electrolyte to have poor wettability on the positive and negative electrodes, prolong the standing time required after the battery cell is filled, and the introduction of ceramic negative electrode coating will increase the interface impedance, which may easily lead to lithium precipitation during the later charging and discharging process. Therefore, there are still safety hazards sometimes. In addition, the materials of inorganic ceramic negative electrode coating are mostly nanoparticles, which will absorb extra water during the production process, which increases the amount of water that needs to be removed during the baking of the electrode, resulting in increased production energy consumption and reduced production efficiency. In addition, the measurement of water will also affect the consistency of the battery. Summary of the invention

[0004] The present application aims to provide a negative electrode coating, a negative electrode and a lithium-ion battery to improve the safety and consistency of the battery.

[0005] The embodiment of the present application is implemented as follows:

[0006] In a first aspect, an embodiment of the present application provides a negative electrode coating formed by curing a coating slurry, wherein the coating slurry includes a binder, an inorganic ceramic, a first organic solvent and an additive, and the additive includes at least one of fluorinated polyethylene, expanded graphite and fluorocarbon wax.

[0007] In one embodiment of the present application, the binder includes at least one of polyvinylidene fluoride, polyacrylonitrile, and polytetrafluoroethylene.

[0008] In one embodiment of the present application, the inorganic ceramic includes at least one of alumina and boehmite.

[0009] In one embodiment of the present application, the first organic solvent includes at least one of N-methylpyrrolidone, γ-butyrolactone, N,N-dimethylformamide, dimethyl carbonate, and ethyl methyl carbonate.

[0010] In one embodiment of the present application, the mass ratio of the binder, the inorganic ceramic, and the additive is in the range of (2-8): (80-90): (2:18).

[0011] In one embodiment of the present application, the solid content of the coating slurry is 15% to 30%.

[0012] In one embodiment of the present application, the thickness of the negative electrode coating is 2 to 20 μm.

[0013] In one embodiment of the present application, the negative electrode coating is prepared by the following steps:

[0014] S1, mixing the binder, the inorganic ceramic, the first organic solvent and the additive to obtain a coating slurry;

[0015] S2, coating the coating slurry on the surface of the negative electrode plate of the lithium ion battery, and drying to form the negative electrode coating.

[0016] In one embodiment of the present application, step S1 includes:

[0017] The binder, the first organic solvent and the additive are first mixed and then allowed to stand for a first period of time to obtain an intermediate slurry; and the inorganic ceramic is then mixed with the intermediate slurry to obtain the coating slurry.

[0018] In one embodiment of the present application, in step S2, the drying method includes: baking in a vacuum drying oven, the baking temperature is 70 to 120° C., and the baking time is 6 to 36 hours.

[0019] In a second aspect, an embodiment of the present application provides a negative electrode, which includes a negative electrode plate and the negative electrode coating described in any one of the first aspects.

[0020] In a third aspect, an embodiment of the present application provides a lithium-ion battery, comprising: a positive electrode; and a negative electrode as described in the second aspect.

[0021] In one embodiment of the present application, the lithium-ion battery further comprises:

[0022] The electrolyte includes a lithium salt, a second organic solvent and a wetting agent, wherein the wetting agent includes at least one of anisole, ethoxybenzene, diphenyl ether, dibenzyl ether, fluorobenzene, furan, ethyl ether, 1,2-dimethylethane, tetrahydrofuran, dibutyl ether, 1,4-dioxane, 1,2-difluorobenzene, 1,3-dioxolane and cyclohexane.

[0023] In one embodiment of the present application, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonylimide), lithium bis(difluorosulfonylimide), and lithium difluorooxalatophosphate.

[0024] In one embodiment of the present application, the second organic solvent includes at least one of dimethyl carbonate, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, fluoroethyl methyl carbonate, tripropyl phosphate, and γ-butyrolactone.

[0025] In one embodiment of the present application, the material of the positive electrode includes at least one of lithium manganese oxide, ternary nickel cobalt lithium manganese oxide or lithium iron phosphate.

[0026] In one embodiment of the present application, the material of the negative electrode includes at least one of graphite and silicon-based materials.

[0027] In one embodiment of the present application, the mixed concentration of the lithium salt and the organic solvent is 0.8-1.5 mol / L.

[0028] In one embodiment of the present application, the mass proportion of the wetting agent in the electrolyte is 3-40wt%.

[0029] Beneficial effects of the technical solution of this application:

[0030] The technical solution of the present application improves the negative electrode coating, alleviates the effect of water absorption of the negative electrode coating on battery consistency, reduces production energy consumption, improves production efficiency, reduces interfacial impedance, inhibits the generation of lithium dendrites, alleviates the problem of lithium desorption, and improves safety performance; and the negative electrode coating is combined with a high-wetting electrolyte to reduce water absorption of the negative electrode, while the wetting and retention of the negative electrode to the electrolyte are greatly improved, reducing battery polarization and further improving safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0032] Figure 1 A schematic diagram of a lithium-ion battery provided in an embodiment of the present application;

[0033] Figure 2 A partial schematic diagram of the negative electrode of a lithium-ion battery provided in an embodiment of the present application.

[0034] Icon: 1000-lithium-ion battery, 100-negative electrode, 110-negative electrode sheet, 120-negative electrode coating, 200-positive electrode. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, rather than all the embodiments. The components of the embodiments of the present application described and shown in the drawings here can be arranged and designed in various different configurations.

[0036] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0037] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0038] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0039] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0040] In the present application, lithium-ion batteries may include lithium-ion secondary batteries, lithium-ion primary batteries, etc. Lithium-ion batteries include one or more battery cells to provide higher voltage and capacity. The battery cell generally includes a shell, a bare battery cell and an electrolyte, and the shell is used to encapsulate the bare battery cell and the electrolyte. The bare battery cell includes a positive electrode sheet, a negative electrode sheet and a diaphragm. The battery cell mainly relies on the movement of metal ions between the positive electrode sheet and the negative electrode sheet to work. The diaphragm is generally a film made of polyethylene (PE) or polypropylene (PP). The diaphragm is used to isolate the positive electrode sheet and the negative electrode sheet, so that the electrons in the battery cannot pass freely, but the ions free in the electrolyte pass through to prevent the positive and negative electrodes from short-circuiting and ensure the smooth progress of the electrochemical reaction.

[0041] In order to improve the energy density and safety of batteries, the positive and negative electrode materials of lithium-ion batteries often select materials with higher gram capacity, and cover the surface of the electrode (such as the positive electrode sheet or the negative electrode sheet) with an inorganic ceramic negative electrode coating in the hope of improving safety performance.

[0042] However, the introduction of inorganic ceramic negative electrode coating will cause the wettability of the electrolyte to the positive and negative electrodes to deteriorate, and the standing time required after the battery cell is injected will be extended. In addition, the electrode sheets need to be dried during the manufacturing process to avoid affecting the wettability of the electrolyte and the electrochemical stability. However, the materials of the inorganic ceramic negative electrode coating are mostly nanoparticles, which will absorb additional water during the production process. This increases the amount of water that needs to be removed during the electrode baking process, resulting in increased production energy consumption and reduced production efficiency. Otherwise, if there is a measure of moisture, it will also affect the consistency of the battery. In addition, the introduction of ceramic negative electrode coating will lead to an increase in interfacial impedance, which is easy to cause lithium precipitation during the later charging and discharging process. Therefore, how to further improve safety and consistency remains one of the key research focuses in this field.

[0043] In view of this, the present application provides a technical solution to improve the negative electrode coating, alleviate the impact of water absorption of the negative electrode coating on battery consistency, reduce production energy consumption, improve production efficiency, reduce interface impedance, inhibit the generation of lithium dendrites, alleviate lithium decomposition problems, and improve safety performance; and, the negative electrode coating is combined with a high-wetting electrolyte to reduce water absorption of the negative electrode, while the wetting and retention of the negative electrode to the electrolyte are greatly improved, reducing battery polarization and further improving safety performance.

[0044] It should be noted that the negative electrode coating in the present application can be applied not only to the negative electrode plate, but also to other structures of the negative electrode, such as the negative electrode column, etc. The present application embodiment is described by taking the plate as an example.

[0045] like Figure 1 As shown, an embodiment of the present application provides a lithium-ion battery 1000 , and the lithium-ion battery 1000 includes a positive electrode 200 and a negative electrode 100 .

[0046] The material of the positive electrode 200 includes at least one of lithium manganese oxide, ternary nickel cobalt lithium manganese oxide or lithium iron phosphate.

[0047] The material of the negative electrode 100 includes at least one of graphite and silicon-based materials.

[0048] like Figure 2 As shown, the negative electrode 100 includes a negative electrode sheet 110 and a negative electrode coating 120 covering the surface of the negative electrode sheet 110 .

[0049] The negative electrode coating 120 is formed by curing a coating slurry, wherein the coating slurry includes a binder, an inorganic ceramic, a first organic solvent, and an additive, wherein the additive includes at least one of fluorinated polyethylene, expanded graphite, and fluorocarbon wax.

[0050] In some embodiments, the thickness of the negative electrode coating 120 is 2-20 μm. Within this thickness range, the negative electrode coating 120 can improve the safety performance and cycle life of the battery, while having a low impact on the energy density and electrochemical performance of the battery.

[0051] In some embodiments, the binder includes at least one of polyvinylidene fluoride, polyacrylonitrile, and polytetrafluoroethylene.

[0052] In some embodiments, the inorganic ceramic includes at least one of alumina and boehmite.

[0053] In some embodiments, the first organic solvent includes at least one of N-methylpyrrolidone, γ-butyrolactone, N,N-dimethylformamide, dimethyl carbonate, and ethyl methyl carbonate.

[0054] In some embodiments, the additive includes at least one of fluorinated polyethylene, expanded graphite, and fluorocarbon wax.

[0055] In some embodiments, the mass ratio of the binder, the inorganic ceramic, and the additive is in the range of (2-8): (80-90): (2:18).

[0056] In some embodiments, the solid content of the coating slurry is 15% to 30%.

[0057] In some embodiments, the negative electrode coating 120 is prepared by the following steps:

[0058] S1, mixing a binder, an inorganic ceramic, a first organic solvent and an additive to obtain a coating slurry;

[0059] S2 , coating the coating slurry on the surface of the negative electrode plate 110 of the lithium-ion battery 1000 , and drying to form a negative electrode coating 120 .

[0060] In some embodiments, step S1 includes:

[0061] S11, mixing a binder, a first organic solvent and an additive, and then standing for a first period of time to obtain an intermediate slurry;

[0062] S12, mixing the inorganic ceramic with the intermediate slurry to obtain a coating slurry. The mixing may be performed by stirring and dispersing with a dispersion disk at a rotation speed of 1500 to 3000 r / min and a stirring time of 0.5 to 3 hours.

[0063] In some embodiments, in step S2, the drying method includes: baking in a vacuum drying oven, the baking temperature is 70 to 120° C., and the baking time is 6 to 36 hours.

[0064] The embodiment of the present application improves the negative electrode coating 120, and the negative electrode coating 120 has hydrophobic and lipophilic properties, which effectively alleviates the problem of water absorption by the negative electrode coating 120, alleviates the adverse effects of water absorption by the negative electrode coating 120 on battery consistency, reduces production energy consumption, and improves production efficiency. At the same time, it gives full play to the characteristics of inorganic ceramic nanoparticles, improves the wetting and retention capabilities of the electrolyte, reduces interfacial impedance, inhibits the generation of lithium dendrites, alleviates the problem of lithium decomposition, and improves safety performance.

[0065] In addition, the lithium ion battery 1000 also has an electrolyte. The electrolyte includes a lithium salt, a second organic solvent and a wetting agent, and the wetting agent includes at least one of anisole, ethoxybenzene, diphenyl ether, dibenzyl ether, fluorobenzene, furan, ethyl ether, 1,2-dimethylethane, tetrahydrofuran, dibutyl ether, 1,4-dioxane, 1,2-difluorobenzene, 1,3-dioxolane, and cyclohexane.

[0066] In some embodiments, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonylimide), lithium bis(difluorosulfonylimide), and lithium difluorooxalatophosphate.

[0067] In some embodiments, the second organic solvent includes at least one of dimethyl carbonate, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, fluoroethyl methyl carbonate, tripropyl phosphate, and γ-butyrolactone.

[0068] The mixed concentration of the lithium salt and the second organic solvent is 0.8 to 1.5 mol / L.

[0069] The mass proportion of the wetting agent in the electrolyte is 3-40wt%.

[0070] The embodiment of the present application provides a highly wettable electrolyte in combination with the aforementioned negative electrode coating 120, thereby greatly reducing the water absorption of the negative electrode 100, and greatly improving the wetting and retention of the electrolyte, reducing battery polarization, and further improving safety performance.

[0071] The present application is described in detail below by means of specific examples, which are only partial examples of the present application and are not intended to limit the present application. The raw materials used in the following examples are all commercially available products unless otherwise specified.

[0072] Example 1

[0073] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, fluorinated polyethylene as the additive, and alumina as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0074] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0075] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0076] (2) NCM811 is used to prepare the positive electrode.

[0077] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0078] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0079] Example 2

[0080] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, fluorinated polyethylene as the additive, and alumina as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0081] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0082] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 7 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0083] (2) NCM811 is used to prepare the positive electrode.

[0084] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0085] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0086] Example 3

[0087] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, fluorinated polyethylene as the additive, and boehmite as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0088] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0089] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 7 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0090] (2) NCM811 is used to prepare the positive electrode.

[0091] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0092] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0093] Example 4

[0094] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, polypropylene as the additive, and alumina as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0095] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0096] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0097] (2) NCM811 is used to prepare the positive electrode.

[0098] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0099] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0100] Example 5

[0101] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, fluorinated polyethylene as the additive, and alumina as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0102] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0103] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0104] (2) NCM811 is used to prepare the positive electrode.

[0105] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is 1,2-difluorobenzene (DFB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% DFB is added thereto.

[0106] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0107] Comparative Example 1

[0108] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, and alumina as the inorganic ceramic. Measure the binder and the inorganic ceramic at a mass ratio of 5:90, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0109] The binder and the first organic solvent are mixed and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate and stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing to obtain a coating slurry.

[0110] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0111] (2) NCM811 is used to prepare the positive electrode.

[0112] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0113] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0114] Comparative Example 2

[0115] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, and fluorinated polyethylene as the additive, and measure the binder and the additive in a mass ratio of 5:5, and measure an appropriate amount of the first organic solvent.

[0116] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry, and then stirred and dispersed at a rotation speed of 2500 r / min for 3 hours to obtain a coating slurry.

[0117] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0118] (2) NCM811 is used to prepare the positive electrode.

[0119] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is lithium hexafluorophosphate (LiPF6), the second organic solvent is ethylene carbonate (EC) or diethyl carbonate (DEC), and the wetting agent is fluorobenzene (FB). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FB is added thereto.

[0120] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0121] Comparative Example 3

[0122] (1) Preparation of negative electrode: Select polyvinylidene fluoride (PVDF) as the binder, N-methylpyrrolidone (NMP) as the first organic solvent, fluorinated polyethylene as the additive, and alumina as the inorganic ceramic. Measure the binder, inorganic ceramic, and additive in a mass ratio of 5:90:5, and measure an appropriate amount of the first organic solvent so that the solid content ratio is 15%.

[0123] The binder, the first organic solvent and the additive are mixed, and then allowed to stand for a first period of time to obtain an intermediate slurry. The inorganic ceramic and the intermediate slurry are then placed in a dispersion plate, stirred and dispersed at a speed of 2500 r / min for 3 hours to achieve uniform mixing, and a coating slurry is obtained.

[0124] A graphite negative electrode was selected as the negative electrode, and a coating slurry was coated on the surface of the graphite negative electrode using a coating machine. The thickness of the negative electrode coating was controlled at 5 μm, and then vacuum baked at 60° C. for 8 hours to obtain a negative electrode sheet.

[0125] (2) NCM811 is used to prepare the positive electrode.

[0126] (3) Preparation of electrolyte: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent. The lithium salt is selected from lithium hexafluorophosphate (LiPF6), the second organic solvent is selected from ethylene carbonate (EC) and diethyl carbonate (DEC), and the wetting agent is selected from fluoroethylene carbonate (FEC). A 1 mol / L LiPF6:EC / DEC (1:1 vol) electrolyte system is prepared, and 3 wt% FEC is added thereto.

[0127] (4) The positive electrode sheet and the negative electrode sheet are loaded into the shell, and the electrolyte is injected to prepare a soft-pack battery. After the injection, the battery is aged at 45°C for 24 hours, left at room temperature for 12 hours, and then formed at 45°C with a formation pressure of 0.8MPa. After the formation is carried out at a rate of 0.1C, the finished battery cell is obtained.

[0128] The internal resistance and performance of the lithium ion batteries of Examples 1-5 and Comparative Examples 1-3 were tested. The test results are shown in Table 1.

[0129] Table 1

[0130] Impedance(mΩ) Discharge capacity at 25℃(mAh / g) Example 1 16.8 192 Example 2 25.2 189 Example 3 17.2 193 Example 4 24.6 190 Example 5 16.6 191 Comparative Example 1 38.9 183 Comparative Example 2 17.6 191 Comparative Example 3 36.5 179

[0131] From Table 1, we can see that:

[0132] Comparing Examples 1-5 with Comparative Examples 1-3, the lithium-ion batteries in Examples 1-5 still have a low internal resistance when inorganic ceramics are added to the negative electrode coating, indicating that the lithium-ion batteries provided by the present application are more efficient, less prone to safety hazards such as lithium deposition, and have improved safety; and the lithium-ion batteries in Examples 1-5 have a higher discharge capacity and better cycle performance. It can be seen that the technical solution of the present application alleviates the problems of longer required standing time and increased interface impedance caused by the poor wettability of the electrolyte to the negative electrode under the condition of adding inorganic ceramics, thereby effectively improving the safety and cycle performance of lithium-ion batteries with better consistency.

[0133] Compared with Example 2, Example 1 shows that the thickness of the negative electrode coating can be changed within a certain range and still have a good improvement effect.

[0134] Comparing Example 1 with Example 3, it is shown that the technical solution of the present application can still achieve a good improvement effect by replacing the inorganic ceramic material within a certain range.

[0135] Compared with Example 4, Example 1 shows that when the additive of the negative electrode coating is changed within a certain selection range, it can still have a good improvement effect.

[0136] Compared with Example 5, Example 1 shows that when the wetting agent in the electrolyte is changed within a certain selection range, it can still have a good lifting effect.

[0137] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A negative electrode coating, characterized in that: The coating slurry is solidified to form the coating slurry, wherein the coating slurry includes a binder, an inorganic ceramic, a first organic solvent and an additive, wherein the additive includes at least one of fluorinated polyethylene, expanded graphite and fluorocarbon wax.

2. The negative electrode coating according to claim 1, characterized in that: The binder comprises at least one of polyvinylidene fluoride, polyacrylonitrile and polytetrafluoroethylene; and / or The inorganic ceramic comprises at least one of alumina and boehmite; and / or The first organic solvent comprises at least one of N-methylpyrrolidone, γ-butyrolactone, N,N-dimethylformamide, dimethyl carbonate, and ethyl methyl carbonate; and / or The mass ratio of the binder, the inorganic ceramic, and the additive is in the range of (2-8): (80-90): (2:18); and / or The solid content of the coating slurry is 15% to 30%.

3. The negative electrode coating according to claim 1, characterized in that The thickness of the negative electrode coating is 2-20 μm.

4. The negative electrode coating according to claim 1, characterized in that The negative electrode coating is prepared by the following steps: S1, mixing the binder, the inorganic ceramic, the first organic solvent and the additive to obtain a coating slurry; S2, coating the coating slurry on the surface of the negative electrode plate of the lithium ion battery, and drying to form the negative electrode coating.

5. The negative electrode coating according to claim 4, characterized in that The step S1 comprises: The binder, the first organic solvent and the additive are first mixed to obtain an intermediate slurry; and the inorganic ceramic is then mixed with the intermediate slurry to obtain the coating slurry.

6. The negative electrode coating according to claim 4, characterized in that In the step S2, the drying method includes: baking in a vacuum drying oven, the baking temperature is 70-120° C., and the baking time is 6-36 hours.

7. A negative electrode, characterized in that It comprises a negative electrode sheet and the negative electrode coating according to any one of claims 1 to 6.

8. A lithium ion battery, characterized in that: include: positive electrode; The negative electrode as claimed in claim 7.

9. The lithium-ion battery according to claim 8, characterized in that: The lithium-ion battery also includes: The electrolyte includes a lithium salt, a second organic solvent and a wetting agent, wherein the wetting agent includes at least one of anisole, ethoxybenzene, diphenyl ether, dibenzyl ether, fluorobenzene, furan, ethyl ether, 1,2-dimethylethane, tetrahydrofuran, dibutyl ether, 1,4-dioxane, 1,2-difluorobenzene, 1,3-dioxolane and cyclohexane.

10. The lithium ion battery according to claim 9, characterized in that: The lithium salt comprises at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium bis(oxalatoborate), lithium difluorooxalatoborate, lithium bis(trifluoromethanesulfonylimide), lithium bis(difluorosulfonylimide), and lithium difluorooxalatophosphate; and / or The second organic solvent comprises at least one of dimethyl carbonate, ethylene carbonate, diethyl carbonate, ethyl methyl carbonate, propylene carbonate, ethyl methyl carbonate fluorocarbonate, tripropyl phosphate, and γ-butyrolactone; and / or The material of the positive electrode includes at least one of lithium manganese oxide, ternary nickel cobalt lithium manganese oxide or lithium iron phosphate; and / or The material of the negative electrode includes at least one of graphite and silicon-based materials; and / or The mixed concentration of the lithium salt and the second organic solvent is 0.8 to 1.5 mol / L; and / or The mass percentage of the wetting agent in the electrolyte is 3-40wt%.

Citation Information

Cited By

  • Polymer composite solid electrolyte, battery and preparation method thereof