Preparation method of zinc ion battery electrolyte additive

By using nanodiamond and dimethyl sulfoxide as electrolyte additives in aqueous zinc-ion batteries, the zinc ion deposition behavior is adjusted, the problems of uneven zinc ion deposition and zinc dendrite growth in zinc-ion batteries are solved, and the battery performance is significantly improved. Cycling stability and electrochemical performance.

CN118748276APending Publication Date: 2024-10-08JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410753148.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

During the charge and discharge process of aqueous zinc-ion batteries, uneven zinc ion deposition, zinc dendrite growth and corrosion problems affect battery performance, leading to reduced zinc anode utilization, reduced Coulombic efficiency and rapid capacity fading, affecting the reversibility and cycle life of the battery.

Method used

Nanodiamonds (NDs) and dimethyl sulfoxide (DMSO) are used as electrolyte additives, and NDs are uniformly dispersed in DMSO through ultrasonic dispersion method to prepare NDs-DMSO-ZS composite electrolyte, adjust the zinc ion deposition behavior, and optimize the electrode-electrolyte interface .

Benefits of technology

It achieves uniform deposition of zinc ions, improves the cycle stability and capacity retention rate of aqueous zinc-ion batteries, significantly improves the electrochemical performance and Coulombic efficiency of the battery, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118748276A_ABST
    Figure CN118748276A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a zinc ion battery electrolyte additive, which belongs to the technical field of zinc ion batteries and is used for improving the performance of a water-based zinc ion battery by taking nano-diamond and dimethyl sulfoxide as electrolyte additives. The nano-diamond / dimethyl sulfoxide electrolyte additive is obtained by adding nano-diamond into dimethyl sulfoxide by utilizing an ultrasonic dispersion method, so that the capacity and the cycling stability of the aqueous zinc ion battery are improved. The nano-diamond / dimethyl sulfoxide is used as an electrolyte additive, so that the surface of the zinc negative electrode is protected. When the nano-diamond / dimethyl sulfoxide is used as the zinc ion battery additive, the assembled symmetric battery, asymmetric battery and total battery have good cycling stability, relatively high coulombic efficiency and good reversible specific capacity and retention rate. The nano-diamond and the dimethyl sulfoxide are used as electrolyte additives, so that the capacity and the cycling stability of the zinc ion battery are improved, and the cost benefit and the industrial prospect are good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of zinc ion batteries and relates to a method for improving the performance of aqueous zinc ion batteries by using nanodiamonds (NDs) and dimethyl sulfoxide (DMSO) as electrolyte additives to synergistically regulate zinc ion deposition behavior. Background Art

[0002] With the growing demand for renewable energy in contemporary society, the optimization of renewable energy production and utilization methods has also been continuously improved. It is imperative to develop large-scale energy storage systems with high energy density, safety and environmental friendliness. Aqueous zinc-ion batteries (AZIBs) have become an important candidate among many solutions due to their advantages such as high theoretical capacity, low redox potential and low production cost. With the continuous development of materials such as electrodes, diaphragms and electrolytes, the performance of AZIBs has been continuously improved, which has also promoted the commercial development of AZIBs. However, problems such as zinc dendrite growth, hydrogen evolution and corrosion will seriously affect the performance of the battery, which is mainly reflected in the reduction of zinc anode utilization, reduced Coulomb efficiency and rapid capacity decay. During the charge and discharge process, zinc ion plating / stripping occurs continuously at the electrode-electrolyte interface, and the zinc deposition uniformity is poor, which affects the reversibility and cycle life of the battery. Therefore, it is necessary to improve the performance of the battery by optimizing the internal structure of the battery. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the background technology and provide a nanodiamond (NDs) and dimethyl sulfoxide (DMSO) as electrolyte additives to obtain an electrolyte with good electrochemical performance, low cost and green environmental protection for improving the performance of aqueous zinc ion batteries.

[0004] The invention adopts an ultrasonic dispersion method to add NDs into DMSO to obtain an NDs-DMSO electrolyte additive, thereby improving the capacity and cycle stability of an aqueous zinc ion battery.

[0005] The technical solution of the present invention is as follows:

[0006] A zinc ion battery electrolyte additive is obtained by uniformly dispersing 1-10 mg of NDs in 1-50 mL of a DMSO organic solvent.

[0007] The particle size of the NDs is preferably 5 to 10 nm.

[0008] Preferably, NDs are 5 mg and DMSO is 5 mL.

[0009] The additive is used for preparing NDs-DMSO-ZS composite electrolyte.

[0010] The preparation method of NDs-DMSO-ZS composite electrolyte is as follows:

[0011] 1) Dissolve 10-15 g of zinc sulfate heptahydrate in 20 mL of deionized water to prepare a 2 M blank ZS electrolyte;

[0012] 2) Adding the zinc ion battery electrolyte additive to the 2M blank ZS electrolyte and adjusting the volume to the required capacity, the NDs-DMSO-ZS composite electrolyte can be obtained;

[0013] Preferably, in step 1), the amount of zinc sulfate heptahydrate is 11.5 g.

[0014] Preferably, in step 2), 1 mL of the zinc ion battery electrolyte additive and 5 mL of the 2M blank ZS electrolyte are taken and the volume is fixed to 6 mL.

[0015] Beneficial effects of the present invention:

[0016] 1. In the samples prepared by the present invention, the NDs have good dispersibility in the composite electrolyte.

[0017] 2. The sample prepared by the present invention has the function of optimizing electrolyte, can adjust the deposition behavior of zinc ions, and realize a uniform zinc deposition layer, and can be used as an ideal electrolyte for aqueous zinc ion batteries.

[0018] 3. The samples prepared by the present invention have excellent electrochemical properties, and the aqueous zinc ion batteries made with them have good cycle stability and capacity retention rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 The Zn||Zn symmetric battery assembled using the NDs-DMSO-ZS composite electrolyte of the embodiment is 2 Scanning electron micrograph of the zinc anode after cycling for 20 h at a current density of 1.5 Å.

[0020] Figure 2 The Zn||Zn symmetric cell assembled using the ZS electrolyte of the embodiment is 2 Scanning electron micrograph of the zinc anode after cycling for 20 h at a current density of 1.5 Å.

[0021] Figure 3 It is the Arrhenius curve of the Zn||Zn symmetric battery assembled using the NDs-DMSO-ZS composite electrolyte of Example and the ZS electrolyte of Example.

[0022] Figure 4 The Zn||Zn symmetric battery assembled using the NDs-DMSO-ZS composite electrolyte and the ZS electrolyte in the embodiment was subjected to a constant current density of 1 mA / cm2 The following cycle performance comparison chart.

[0023] Figure 5 The Zn / / Cu asymmetric battery assembled using the NDs-DMSO-ZS composite electrolyte and the ZS electrolyte of the embodiment is 2 Comparison of Coulombic efficiency at different current densities.

[0024] Figure 6 This is a comparison chart of the cycling performance of a Zn / / MnO2 full cell assembled using the NDs-DMSO-ZS composite electrolyte of Example 1 and the ZS electrolyte of Example 1 at a current density of 1 A / g. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be pointed out that the embodiments described below are intended to facilitate the understanding of the present application and do not have any limiting effect thereon.

[0026] Example 1: Preparation of NDs-DMSO-ZS composite electrolyte:

[0027] The NDs (5 mg) prepared by the detonation method were first subjected to a constant temperature drying treatment, and then the dried NDs and DMSO organic solvent (5 mL) were added to a beaker and ultrasonically dispersed for 1 hour to obtain NDs-DMSO electrolyte additive;

[0028] Weigh 11.502g of zinc sulfate heptahydrate and dissolve it in 20mL of deionized water, stir at room temperature until zinc sulfate and heptahydrate are completely dissolved to prepare 2M blank ZS electrolyte. Then add the obtained NDs-DMSO (1mL) electrolyte additive to 2M blank ZS electrolyte (5mL) to prepare NDs-DMSO-ZS composite electrolyte.

[0029] In this embodiment, the drying and evaporation were carried out at a constant temperature of 60° C., the ultrasonic treatment time was 1 hour, the weighed zinc sulfate and heptahydrate were not further treated, and all the operations were carried out at room temperature.

[0030] Example 2: Preparation of ZS electrolyte:

[0031] This example is a comparative example, which is a prior art. The prepared sample is used for performance comparison with the sample prepared by the NDs-DMSO-ZS composite electrolyte (method of the present invention) in Example 1 to illustrate the effect of the present invention.

[0032] 11.5 g of zinc sulfate heptahydrate was weighed and dissolved in 20 mL of deionized water, and stirred at room temperature until the zinc sulfate heptahydrate was completely dissolved to prepare a 2M blank ZS electrolyte. In this embodiment, the weighed zinc sulfate heptahydrate was not further processed, and all operations were performed at room temperature.

[0033] Example 3: Using MnO2 material to make a positive electrode for a zinc ion battery

[0034] The Zn||Zn symmetrical battery, Zn / / Cu asymmetric battery, and Zn / / MnO2 full battery use pure zinc and copper, commercial Whatman GF glass fiber separator, and use a special cutting die to cut the pure zinc and copper into several electrode discs with a diameter of 12 mm, and use a special cutting die to cut the separator into discs with a diameter of 16 mm.

[0035] The positive electrode of the Zn / / MnO2 full battery is composed of 70wt% commercial MnO2 material (active substance), 10wt% binder (polyvinylidene fluoride, PVDF) and 20wt% conductive agent Super P. The three are mixed and ground for 30 minutes and then put into a container. 10-12 drops of 1-methyl-2-pyrrolidone (NMP, solvent) are added to the container and then placed on a magnetic stirrer and stirred at a uniform speed for 6 hours until the mixture becomes a viscous fluid. Using carbon paper as the current collector, apply the above mixed viscous material on the carbon paper, and the coating density must be uniform. Set the temperature of the vacuum drying oven to 80°C, take the above carbon paper coating and place it in the vacuum drying oven. After timing for 12 hours, take it out for use. Use a special cutting knife mold to cut the prepared carbon paper coating into several electrode discs with a diameter of 12mm.

[0036] Example 4: Preparation and performance testing of zinc ion batteries

[0037] Sample ZS and sample NDs-DMSO-ZS are used as electrolytes for aqueous zinc ion batteries. The amount of electrolyte can be controlled at 150μL. The two electrolytes are added in exactly the same way to test their performance in zinc ion batteries. The zinc ion battery prepared in this test is a CR-2025 button battery. Then weigh the mass of the electrode sheet to prepare for the calculation of subsequent specific capacity parameters. Take the matching battery positive and negative electrode shells, gaskets, shrapnel, Whatman GF glass fiber diaphragm, electrolyte, electrode sheet, etc. and operate them safely and orderly according to the production regulations of zinc ion batteries to encapsulate the battery. Assemble Zn||Zn symmetric batteries, Zn / / Cu asymmetric batteries, and Zn / / MnO2 full batteries with sample ZS and sample NDs-DMSO-ZS electrolytes.

[0038] Example 5: Performance test of different zinc ion batteries

[0039] The LAND battery test system (CT2001 1A) was used to test the Zn||Zn symmetric battery, Zn / / Cu asymmetric battery and Zn / / MnO2 full battery. At 25°C, the battery was discharged to 0.8V at a certain current density; after the discharge, it was charged to 1.9V at a certain current density; after the charge, it was discharged to 0.8V at the same current density, and the cycle was repeated for constant current cycle test. The electrochemical workstation was used to test the electrochemical impedance spectrum (EIS) of the Zn||Zn symmetric battery. The frequency range was set to 100kHz to 0.01Hz, the temperature was from 45°C to 65°C, and the average was recorded once at each point at 5°C, which was used to calculate the activation energy of the Zn||Zn symmetric battery under different electrolytes.

[0040] Effect verification:

[0041] 1) Characterization of the Zn anode surface using NDs-DMSO-ZS electrolyte

[0042] The Zn||Zn symmetric battery was investigated by scanning electron microscopy (SEM) at 1 mA / cm 2 The zinc anode was characterized after cycling for 20 hours at the current density. Figure 1 As shown in Figure 2, the surface of the zinc anode using the NDs-DMSO-ZS composite electrolyte is smooth and no obvious zinc dendrites appear. This is attributed to the optimization effect of the NDs-DMSO additive on the electrolyte, which promotes the uniform deposition of zinc ions and reduces zinc dendrites and byproducts.

[0043] 2) Characterization of the Zn anode surface using ZS electrolyte

[0044] The Zn||Zn symmetric battery was investigated by scanning electron microscopy (SEM) at 1 mA / cm 2 The zinc anode was characterized after cycling for 20 hours at the current density. Figure 2 As shown in Figure 2, the surface of the zinc anode using the ZS electrolyte is covered with many micron-sized flakes and protrusions, indicating that a large number of zinc dendrites have been generated on its surface. This is mainly due to the uneven deposition of zinc ions, which leads to the formation of zinc dendrites and byproducts.

[0045] 3) Electrochemical workstation tests the impedance of Zn||Zn symmetric cells with different electrolytes

[0046] The impedance spectra (EIS) of the Zn||Zn symmetric cells of the two electrolytes were tested at different temperatures (45℃-65℃) using an electrochemical workstation. The desolvation activation energy of the two Zn||Zn symmetric cells was calculated using the obtained impedance. The results are as follows: Figure 3Arrhenius curve. The desolvation activation energy of the Zn||Zn symmetric cell using the NDs-DMSO-ZS composite electrolyte is 43.86KJ / mol, and the desolvation activation energy of the Zn||Zn symmetric cell using the ZS electrolyte is 57.62KJ / mol. Generally speaking, lower activation energy values ​​are conducive to promoting the desolvation process of hydrated zinc ions. From the comparison results obtained, the activation energy value of the Zn||Zn symmetric cell using the NDs-DMSO-ZS electrolyte is the smallest, indicating that the NDs-DMSO additive has a positive effect on the kinetics of the zinc plating process.

[0047] 4) Battery testing system tests Zn||Zn battery

[0048] The LAND battery test system (CT2001 1A) was used to test the two Zn||Zn symmetric batteries at 1 mA / cm 2 Current density, specific capacitance is 1 mAh / cm 2 The constant current cycle test is carried out under Figure 4 As shown in the figure, the cycle life of the Zn||Zn symmetric battery using the NDs-DMSO-ZS composite electrolyte is close to 1500 hours, which is much longer than the Zn||Zn symmetric battery with the ZS electrolyte (342 hours). This shows that the NDs-DMSO additive is beneficial to the battery cycle stability. This can be attributed to the hydrogen bonds formed between NDs and DMSO and water molecules, which regulate the deposition kinetics of zinc ions and facilitate the uniform deposition of zinc ions.

[0049] 5) Battery testing system tests Zn / / Cu batteries

[0050] The LAND battery test system (CT2001 1A) was used to test the two Zn / / Cu asymmetric batteries at 2 mA / cm 2 Current density, specific capacitance is 1 mAh / cm 2 The effects of two electrolytes on the reversible behavior of Zn / / Cu asymmetric batteries were studied. Figure 5 As shown in the figure, the Zn / / Cu asymmetric battery using the NDs-DMSO-ZS composite electrolyte can be cycled for more than 800 hours with an average Coulombic efficiency (CE) of up to 99.8%. In contrast, the Zn / / Cu asymmetric battery using the ZS electrolyte exhibited significant CE fluctuations throughout the cycle and cycled for less than 200 hours, indicating that side reactions and dendrites formed, leading to irreversible cycling of the battery.

[0051] 6) Battery testing system tests Zn / / MnO2 batteries

[0052] The LAND battery test system (CT2001 1A) was used to test the two Zn / / MnO2 batteries at a current density of 1A / g (mass loading of 2.1mg / cm 2 ) under the condition of full battery, the long-term cycle stability was evaluated. Figure 6 As shown, the Zn / / MnO2 full battery using the NDs-DMSO-ZS composite electrolyte still has a high reversible capacity of 80.8mAh / g after 2000 cycles. In contrast, the Zn / / MnO2 full battery using the ZS electrolyte has a lower reversible specific capacity during the entire cycle. The improvement in battery performance is attributed to the optimization of the electrolyte by NDs and DMSO, which adjusts the deposition behavior of zinc ions, is conducive to inhibiting the generation of zinc dendrites and side reactions, and ensuring the continuous cycle stability of aqueous zinc-ion batteries.

[0053] When the sample NDs-DMSO prepared by the method of the present invention is used as an electrolyte additive for aqueous zinc ion batteries, the prepared Zn||Zn symmetrical battery has extremely high cycle stability. The analysis of the zinc anode surface morphology using a scanning electron microscope also shows that there are no obvious flaky zinc dendrites on the zinc anode surface, indicating that the NDs-DMSO additive has a good regulation of the zinc ion deposition behavior at the electrode-electrolyte interface and plays a certain protective role on the zinc anode surface. When the sample NDs-DMSO prepared by the method of the present invention is used as an additive for zinc ion batteries, the prepared Zn||Zn symmetrical battery and Zn / / Cu asymmetric battery have good cycle stability and high coulomb efficiency; the prepared Zn / / MnO2 full battery has a good reversible specific capacity and retention rate, showing that the material prepared by the present invention has excellent electrochemical properties.

Claims

1. A zinc ion battery electrolyte additive, characterized in that The additive is obtained by uniformly dispersing 1-10 mg of nano-diamond in 1-50 mL of an organic solvent, dimethyl sulfoxide.

2. The zinc ion battery electrolyte additive according to claim 1, characterized in that The particle size of the nano diamond is 5-10nm.

3. The zinc ion battery electrolyte additive according to claim 1, characterized in that The amount of nanodiamond is 5 mg, and the amount of dimethyl sulfoxide is 5 mL.

4. Use of the zinc ion battery electrolyte additive according to any one of claims 1 to 3 for preparing NDs-DMSO-ZS composite electrolyte.

5. The use of the zinc ion battery electrolyte additive according to claim 4, characterized in that: The preparation method of NDs-DMSO-ZS composite electrolyte is as follows: 1) Dissolve 10-15 g of zinc sulfate heptahydrate in 20 mL of deionized water to prepare a 2 M blank ZS electrolyte; 2) Add the zinc ion battery electrolyte additive to the 2M blank ZS electrolyte and adjust the volume to the required capacity to obtain the NDs-DMSO-ZS composite electrolyte.

6. The use of the zinc ion battery electrolyte additive according to claim 5, characterized in that: In step 1), the amount of zinc sulfate heptahydrate is 11.5 g.

7. The use of the zinc ion battery electrolyte additive according to claim 5, characterized in that: In step 2), 1 mL of zinc ion battery electrolyte additive and 5 mL of 2M blank ZS electrolyte were taken and the volume was fixed to 6 mL.