Nonlinear Hall rectifier based on N-type tellurium elementary substance semiconductor and preparation method thereof
By fabricating an N-type tellurium nanosheet nonlinear Hall rectifier and using alumina to adjust the carrier concentration and back gate voltage, the problem of the difficulty in controlling P-type tellurium elemental semiconductors to N-type was solved, achieving a high-performance nonlinear Hall rectification effect suitable for industrial production.
Patent Information
- Application Number
- CN202410785257.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-08
AI Technical Summary
Existing technologies make it difficult to modulate P-type tellurium semiconductors into N-type semiconductors, which limits the performance of the nonlinear Hall effect and makes it difficult to achieve high-performance rectification at room temperature.
Tellurium nanosheets were prepared by hydrothermal method, and nickel-gold contact electrodes were grown on the tellurium nanosheets by combining electron beam photomasking and magnetron sputtering technology. The nanosheets were then covered with an aluminum oxide film. By adjusting the carrier concentration and applying the back gate voltage, the Fermi level of the N-type tellurium was brought close to the bottom of the conduction band, thereby enhancing the nonlinear Hall rectification effect.
The fabricated N-type tellurium nanosheet nonlinear Hall rectifier exhibits high-performance rectified voltage response in the low-temperature to room-temperature range, with a rectified voltage response of up to 1.7 × 10⁶ V/W, making it suitable for industrial production.
Smart Images

Figure CN118748907A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nonlinear electronic devices, and in particular to a nonlinear Hall rectifier based on an N-type tellurium single-element semiconductor and a preparation method thereof. Background Art
[0002] The Hall effect is a typical linear electrical transport phenomenon. When the system breaks the time reversal symmetry, there is a linear relationship between the applied current and the generated Hall voltage. In recent years, the corresponding second-order nonlinear Hall effect has attracted widespread attention. The nonlinear Hall voltage is linearly related to the square of the current, and it can still exist in a system with time reversal symmetry, but it is necessary to break the spatial inversion symmetry. Utilizing the parabolic IV characteristics, when an alternating current is added, the nonlinear Hall effect can simultaneously generate a doubled frequency resonant voltage and a rectified DC voltage, and can be used as a nonlinear Hall rectifier in industrial production. Unlike traditional diode-type rectifiers, nonlinear Hall rectifiers do not rely on junction or barrier structures, so the sample has a larger proportion of available working area and a smaller power threshold.
[0003] Symmetry is the most important parameter for regulating the nonlinear Hall effect. Elemental tellurium is a chiral topological crystal that lacks spatial symmetry, has spin-orbit coupling, and has a KramersWeyl point at the bottom of the conduction band, making it an ideal candidate material for nonlinear Hall. Tellurium is a natural P-type semiconductor with a Fermi level in the valence band. In order to obtain a larger nonlinear Hall effect, it is necessary to adjust the Fermi level to near the bottom of the conduction band by doping electrons. It is difficult to regulate tellurium into an N-type semiconductor by adding a back-gate voltage without intervention. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention proposes a nonlinear Hall rectifier based on an N-type tellurium single-element semiconductor and a preparation method thereof. The rectifier of the present invention relies on the resonant signal and rectification signal generated by the nonlinear Hall effect. After being adjusted by aluminum oxide, the P-type tellurium can be adjusted to N-type tellurium. Further, by applying a back gate voltage, the Fermi level is close to the Weyl point at the bottom of the conduction band, and a strong nonlinear Hall rectification signal is obtained. The rectifier of the present invention is a high-performance nonlinear Hall rectifier device that can operate in the low temperature to room temperature range. It exhibits a very high performance rectification voltage response at room temperature, which can reach 1.7×10 6 V / W.
[0005] The present invention adopts the following technical solutions.
[0006] The present invention provides a method for preparing a nonlinear Hall rectifier based on an N-type tellurium single-element semiconductor, comprising the following steps:
[0007] (1) Using sodium tellurite and water as the tellurium source and solvent, respectively, in the presence of a reducing agent, a template agent, and aqueous ammonia, tellurium nanosheets were prepared by a hydrothermal method;
[0008] (2) coating a solution containing tellurium nanosheets on a substrate;
[0009] (3) Through the electron beam mask process, relying on electron beam exposure and argon ion etching technology, tellurium nanosheets are made into Hall strip devices;
[0010] (4) growing nickel and gold as contact electrodes on the sides of the tellurium Hall strip device by physical vapor deposition;
[0011] (5) A magnetron sputtering growth method is used to cover the surface of the Hall strip device with an aluminum oxide film to adjust the carrier concentration and prevent device degradation, thereby obtaining a nonlinear Hall rectifier based on an N-type tellurium semiconductor; when the aluminum oxide is grown by magnetron sputtering, the growth temperature is between room temperature and 50°C, and the growth rate is less than 1.2nm / min.
[0012] In the present invention, the thickness of the tellurium nanosheets on the substrate is 20-50nm, and the thickness of the aluminum oxide film grown by magnetron sputtering is 15-50nm; in order to reduce the potential barrier between the electrode and the tellurium contact point, metal nickel with a suitable work function is selected as a buffer layer. In order to make the nickel fully contact the tellurium nanosheets, the thickness of the nickel electrode should be close to or equal to the thickness of the tellurium nanosheets, which is 20-50nm, and the thickness of the gold electrode is greater than 20nm.
[0013] In the present invention, in step (1), the reducing agent is hydrated hydrazine, the template agent is polyvinyl polypyrrolidone (PVP), the hydrothermal reaction temperature is 175-185° C., and the hydrothermal reaction time is 3-5 hours.
[0014] In the present invention, in step (2), the solution containing tellurium nanosheets is an ethanol solution; during coating, the solution is dropped onto a pre-cleaned substrate, and the droplets are blown dry with a nitrogen gun to form a tellurium nanosheet structure on the substrate; the substrate is a silicon substrate, which is a two-layer structure, the lower layer is highly doped conductive silicon, and the upper layer is insulating silicon dioxide;
[0015] In the present invention, in step (3), PMMA A4 electron beam positive resist is spin-coated on the substrate, and then the tellurium thin film is etched into a Hall strip shape by electron beam exposure and argon ion etching technology, and the electron beam resist is washed away after the etching is completed; in step (4), MMA EL6 and PMMA A4 double-layer electron beam resist are spin-coated on the substrate in sequence, and the electrode composition is etched by electron beam exposure, and then metal nickel and gold are deposited, and finally the excess electron beam resist is removed to form a contact electrode.
[0016] In the present invention, in step (4), the physical vapor deposition method is magnetron sputtering.
[0017] In the present invention, in step (5), the room temperature is the ambient temperature, which is between 5°C and 30°C, and the growth rate is 0.5-1 nm / min.
[0018] The present invention also provides a nonlinear Hall rectifier based on N-type tellurium nanosheets prepared by the above-mentioned preparation method, which includes a substrate, tellurium nanosheets on the substrate, nickel and gold contact electrodes above the tellurium nanosheets, and an aluminum oxide film layer covering the entire device.
[0019] In the present invention, the substrate is a silicon substrate, which is a two-layer structure, the lower layer is highly doped conductive silicon, and the upper layer is insulating silicon dioxide; the thickness of the tellurium nanosheet is 20-50nm, and the excessive thickness of the nanosheet weakens the ability of aluminum oxide to adjust the carrier concentration, and the P-type tellurium nanosheet cannot be adjusted to N-type; the thickness of the aluminum oxide film is 15-50nm. In a specific embodiment, the thickness of the aluminum oxide film is 28nm, the thickness of the nickel electrode is 20nm, and the thickness of the gold electrode is 60nm.
[0020] Furthermore, the present invention provides a method for regulating the rectifier voltage response of the nonlinear Hall rectifier based on the N-type tellurium nanosheets, wherein the alternating current is applied along the direction of the Hall strip, and the rectified DC voltage is measured along the Hall direction; the carrier concentration is regulated by the aluminum oxide film on the tellurium surface or regulated under the action of the back gate voltage to improve the rectifier voltage response. When the back gate voltage regulation is added, the rectifier voltage response of the N-type tellurium is the largest.
[0021] In the present invention, the operating temperature of the rectifier is between 10-300K. Too high an operating temperature will cause tellurium to melt and damage the device.
[0022] The preparation method of the present invention includes hydrothermal growth of tellurium nanosheets, micro-nano process to make the sample into Hall strips, evaporation of nickel / gold as contact electrodes, and overall coverage with aluminum oxide film for carrier concentration adjustment and device protection; the present invention can enhance the effect of carrier doping by increasing the growth temperature of aluminum oxide, changing the growth rate, and increasing the thickness of aluminum oxide. Compared with the prior art, the present invention has the following beneficial effects:
[0023] In the device of the present invention, by controlling the thin film growth conditions to grow aluminum oxide and adjust the carrier concentration, P-type tellurium is converted into an N-type semiconductor. Further, by applying a back gate voltage, the Fermi level of tellurium can be adjusted to the bottom of the conduction band near the Weyl point, thereby generating an enhanced nonlinear Hall rectification effect, so that the rectifier has good rectification performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is an optical micrograph of a tellurium sheet and a Hall strip according to an embodiment of the present invention.
[0025] Figure 2This is a schematic diagram of the measurement of nonlinear Hall and rectification effects.
[0026] Figure 3 The back gate voltage regulates the rectifier under the condition of different growth rates of aluminum oxide; the rectifier resistivity a) and Hall coefficient b) change with the back gate voltage when the aluminum oxide growth rate is 0.7nm / min. At this time, the back gate voltage can adjust the tellurium nanosheet to N-type, that is, the resistivity reaches the maximum value, and the Hall coefficient changes from positive to negative. c) The rectifier resistivity changes with the gate voltage when the aluminum oxide growth rate is 4nm / min. At this time, the tellurium nanosheet is always P-type, that is, the resistivity increases with the increase of positive back gate voltage.
[0027] Figure 4 This is the second-order resonant voltage and rectified voltage generated by the nonlinear Hall effect at low temperature.
[0028] Figure 5 The optimal rectification voltage response and corresponding resistivity are obtained by adjusting the gate voltage at room temperature.
[0029] Figure 6 The voltage response of the N-type tellurium rectifier obtained at different temperatures is compared with other rectifiers. DETAILED DESCRIPTION
[0030] In order to make the technical solution of the present invention clearer, the following is further described in detail with reference to the accompanying drawings and embodiments. It should be understood that the embodiments described below are only used to explain the present invention and are not used to limit the present invention.
[0031] The following describes some of the possible embodiments of the present invention, which is intended to provide a basic understanding of the present invention, but is not intended to identify the key or decisive elements of the present invention or to limit the scope of protection claimed.
[0032] Example 1
[0033] The present invention provides a high-performance rectifier based on the nonlinear Hall effect of an N-type single-element tellurium semiconductor, wherein the overall structure includes a silicon wafer substrate, a 28nm thick tellurium nanosheet, a nickel / gold electrode, a 20nm thick aluminum oxide film, etc. Among them, the aluminum oxide film is used to adjust the carrier concentration and prevent device degradation. The preparation method is as follows: a solution containing tellurium nanosheets is prepared by a hydrothermal method, and the solution is diluted and spin-coated on the surface of a silicon wafer substrate to obtain a controllably prepared tellurium nanosheet; by an electron beam gel mask process, the tellurium nanosheet is engraved into a Hall strip shape using electron beam exposure and argon ion etching technology; the electron beam gel mask process is used again, and 20nm nickel and 60nm gold are sequentially grown as contact electrodes by magnetron sputtering; finally, 20nm aluminum oxide is grown as a covering layer on the surface of the device by magnetron sputtering to adjust the carrier concentration and protect the device.
[0034] In terms of electrical measurement, a current source is used to apply an AC current to the device, and a DC voltmeter is used to measure the lateral rectified DC voltage. Through the back gate voltage, electrons are filled into the device, thereby adjusting the Fermi level to near the Weyl point at the bottom of the conduction band to obtain the optimal rectified voltage response.
[0035] The silicon wafer used in the present invention has two layers, the lower layer is highly doped conductive silicon, and the upper layer is 285nm thick insulating silicon dioxide. The silicon wafer is ultrasonically cleaned in acetone, isopropanol, and alcohol for 10 minutes using an ultrasonic machine to clean surface impurities, and is subsequently used to transfer tellurium nanosheets.
[0036] Sodium tellurite is used as a raw material, hydrated hydrazine is a reducing agent, and polyvinyl polypyrrolidone PVP is used as a nanosheet molding (structure guide) to make tellurium nanosheets. First, 1.5g of PVP and 46mg of sodium tellurite are dissolved in 1.6ml of deionized water, stirred, 1.66ml of ammonia (25-28%) and 0.84ml of hydrated hydrazine are added halfway, and stirred until the liquid is completely dissolved and clarified. The solution is transferred into a 25ml polytetrafluoroethylene-lined hydrothermal autoclave and kept at a temperature of 180°C for 4 hours. Finally, the obtained cooled product is purified and washed three times with deionized water by centrifugation at 3000rpm, 5000rpm and 8000rpm for 5 minutes respectively. After washing and purification, the silver-gray product is redissolved in ethanol, and the solution is dripped onto a pre-cleaned silicon wafer using a dropper, and the droplets on the silicon wafer are blown dry with a nitrogen gun to obtain tellurium nanosheets for subsequent device production. Tellurium nanosheets are 10-30μm in size and can be stored for about a week in a dry environment, but are easily oxidized in a wet environment.
[0037] After the Te nanosheets grown by the hydrothermal method are transferred to the silicon wafer substrate, they are used to make the rectifier. A drop of PMMA A4 electron beam positive resist is added to the substrate, and the photoresist is rotated at 600r / s and 4000r / s for 6s and 40s respectively, so as to form an electron beam positive resist with a thickness of about 200nm on the silicon wafer substrate. The tellurium thin film is etched into a Hall strip using electron beam exposure and argon ion etching technology. After etching, the electron beam glue was washed off with acetone, and the substrate was covered with MMA EL6 and PMMA A4 double-layer electron beam glue at 600r / s and 4000r / s for 6s and 40s respectively. Electrode patterning was performed by electron beam exposure, and metal electrodes were deposited by magnetron sputtering. 20 / 60nm Ni / Au was used as the electrical contact material for N-type tellurium. Excess electron beam glue was removed by soaking in 60℃ hot acetone for 30min to form contact electrodes for subsequent rectification measurements. Finally, a 20nm aluminum oxide capping layer was deposited on the substrate at a rate of 0.7nm / min at room temperature (ambient temperature) by magnetron sputtering to adjust the carrier density and prevent device degradation, and the rectifier device was completed. Figure 1 Optical photographs of the synthesized tellurium nanosheets and the final rectifier.
[0038] In the physical property measurement system (PPMS, Quantum Design), the nonlinear Hall effect is measured using the traditional four-probe method. The measurement is performed under zero magnetic field. A sinusoidal AC signal I with an amplitude of I and a frequency of ω / 2π is ω =Isinωt is applied to the Hall strip device from a source meter (Keithley 6221), and the first and second harmonic AC voltages are measured simultaneously in the direction parallel to the current and perpendicular to the current (Hall direction) through four lock-in amplifiers (StanfordResearch SR830). For the first and second harmonic measurements, the phases of the lock-in amplifiers are set to 0° and 90° respectively. The rectified DC voltage is measured by a nanovoltmeter (Keithley 2182A). The measurement wiring diagram is as follows Figure 2 To adjust the Fermi level to the conduction band region, silver paste was applied to the bottom of the silicon wafer as the positive gate voltage, the negative electrode of the current meter was connected to the negative gate voltage, and a sub-microampere programmable source meter (Keithley 6430) was used to apply the back gate voltage and measure the leakage current.
[0039] For comparison, the present invention fabricated a rectifier with a 20 nm aluminum oxide capping layer deposited on a substrate at a rate of 4 nm / min. Figure 3 As shown in Figure 1, the aluminum oxide deposited at a rate of 0.7 nm / min can provide the function of doping carriers. At this time, the back gate voltage can adjust the Fermi level to cross the middle of the band gap (at this time, the resistivity reaches the maximum value), and the tellurium nanosheet changes from P-type to N-type. At this time, the Hall coefficient R H From positive to negative. Aluminum oxide deposited at a rate of 4nm / min can only provide a protective layer. The back gate voltage cannot adjust the Fermi level to the middle of the band gap by means of electron doping, the resistivity cannot reach the peak value, and the tellurium nanosheet cannot be converted from P-type to N-type.
[0040] When an alternating current is passed through the device, a resonant voltage signal with a parabolic relationship with the current can be obtained due to the nonlinear Hall effect of the material. and rectified DC voltage signal like Figure 4 As shown, since the lock-in amplifier measures the effective value of the alternating signal, the ratio of the rectified voltage signal to the second-order resonant voltage signal is approximately
[0041] The magnitude of the nonlinear Hall effect can be determined by the nonlinear Hall conductivity Characterization, where σ xx is the sample conductivity, is the voltage parallel to the direction of current, is the nonlinear Hall voltage, L and W are the length and width of the device respectively. The magnitude of the rectification effect can be determined by the voltage response. characterization, t is the device thickness. By adding back gate voltage, the position of the Fermi level can be adjusted to control the electrical properties of the device to the optimal state. Figure 5 As shown in Figure 1, when a positive gate voltage is applied, electrons are doped into the device, the Fermi level is shifted to the conduction band, and the rectifier voltage response increases. When the optimal performance is achieved, the device conductance is σ xx =104S / m, high nonlinear Hall conductivity, 0.019A / V 2 , the device conductivity is small and the nonlinear Hall conductivity is high, then the rectifier has a high voltage response R v =1.7×10 6 V / W. Figure 6 As shown, the star shape is the result of the rectifier of the present invention, and the rectifier voltage response is greatly improved compared with other materials or structures. (Nat. Nanotechnol. 16 (4), 421-425 (2021); Nat. Commun. 10 (1), 1290 (2019); Nat. Commun. 14 (1), 364 (2023); Nat. Commun. 7, 11670 (2016); Nat. Mater. 13, 50-56 (2014); IEEE Transactions on Microwave Theory and Techniques 62, 965-976 (2014); Nature 565,337-342(2019); Nat.Mater.18,324-328(2019); Phys.Rev.Lett.129,186801(2022); Nat.Nanotechnol.17,378-383(2022); Nat.Commun.13(1),546 5(2022); Nature.621(7979),487-492(2023); Chin.Phys.Lett.38(1),017301(2021); Nat.Commun.14(1),364(2023); Nat.Commun.15(1),245(2024).).
Claims
1. A method for preparing a nonlinear Hall rectifier based on an N-type tellurium semiconductor. It is characterized in that The following steps are involved: (1) Using sodium tellurite and water as the tellurium source and solvent, respectively, in the presence of a reducing agent, a template agent, and aqueous ammonia, tellurium nanosheets were prepared by a hydrothermal method; (2) coating a solution containing tellurium nanosheets on a substrate; (3) Through the electron beam mask process, relying on electron beam exposure and argon ion etching technology, the tellurium nanosheets are made into Hall strip devices; (4) growing nickel and gold as contact electrodes on the sides of the tellurium Hall strip device by physical vapor deposition; (5) A magnetron sputtering growth method is used to cover the surface of the Hall strip device with an aluminum oxide film to adjust the carrier concentration and prevent device degradation, thereby obtaining a nonlinear Hall rectifier based on an N-type tellurium semiconductor; when the aluminum oxide film is grown by magnetron sputtering, the growth temperature is between room temperature and 50°C, and the growth rate is less than 1.2nm / min.
2. The preparation method according to claim 1, It is characterized in that In step (1), the reducing agent is hydrated hydrazine, the template agent is polyvinyl polypyrrolidone (PVP), the hydrothermal reaction temperature is 175-185° C., and the hydrothermal reaction time is 3-5 hours.
3. The preparation method according to claim 1, It is characterized in that In step (2), the solution containing tellurium nanosheets is an ethanol solution; when coating, the solution is dropped onto a pre-cleaned substrate, and then the droplets are blown dry with a nitrogen gun; the substrate is a silicon substrate, which has a two-layer structure, the lower layer is highly doped conductive silicon, and the upper layer is insulating silicon dioxide.
4. The preparation method according to claim 1, It is characterized in that In step (3), PMMA A4 electron beam positive resist is dripped onto the substrate, and then the tellurium nanosheets are etched into Hall strips by electron beam exposure and argon ion etching technology. After the etching is completed, the electron beam resist is washed away; in step (4), MMA EL6 and PMMA A4 double-layer electron beam resist are spin-coated on the silicon wafer containing the tellurium nanosheets in sequence, the electrode composition is etched by electron beam exposure, and then metal nickel and gold are deposited. Finally, the excess electron beam resist is removed to form a contact electrode.
5. The preparation method according to claim 1, It is characterized in that In step (4), the physical vapor deposition method is magnetron sputtering.
6. The preparation method according to claim 1, It is characterized in that In step (5), the room temperature is the ambient temperature, which is between 5°C and 30°C, and the growth rate is 0.5-1 nm / min.
7. A nonlinear Hall rectifier based on N-type tellurium nanosheets prepared according to the preparation method of any one of claims 1 to 6, It is characterized in that The device comprises a substrate, tellurium nanosheets on the substrate, nickel and gold contact electrodes above the tellurium nanosheets, and an aluminum oxide film layer covering the entire device.
8. The nonlinear Hall rectifier based on N-type tellurium nanosheets according to claim 7, It is characterized in that The substrate is a silicon substrate with two layers, the lower layer is highly doped conductive silicon, and the upper layer is insulating silicon dioxide; the thickness of the tellurium nanosheets on the substrate is 20-50nm, and the thickness of the aluminum oxide film is 15-50nm.
9. A method for regulating the rectification voltage responsiveness of the nonlinear Hall rectifier based on N-type tellurium nanosheets according to claim 7, It is characterized in that The alternating current is applied along the direction of the Hall strip, and the rectified DC voltage is measured along the Hall direction; the carrier concentration is adjusted by the aluminum oxide film on the tellurium surface or controlled under the action of the back gate voltage to improve the rectified voltage responsiveness.
10. The method according to claim 9, It is characterized in that The operating temperature is between 10-300K.