Polyimide film for graphite sheet, graphite sheet, and method for producing same

By using polyimide films with orientation-disturbing acid anhydrides, diamines, and organic phosphorus compounds in the manufacture of graphite sheets, the problems of low density and productivity of thick graphite sheets have been solved, and the preparation of graphite sheets with high density and efficient heat dissipation has been achieved. .

CN118749012APending Publication Date: 2024-10-08KANEKA CORP

Patent Information

Application Number
CN202380023105.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-25
Filing Date
2023-02-06
Publication Date
2024-10-08

AI Technical Summary

Technical Problem

The existing technology has problems in terms of density and productivity when manufacturing graphite sheets. Especially when preparing thick graphite sheets, surface foaming and reduced thermal conductivity are prone to occur, and the heating rate needs to be reduced to suppress exhaust gas, resulting in poor productivity. reduce.

Method used

By using appropriate amounts of acid anhydrides and diamines that disrupt orientation as raw materials for polyimide films, heat treatment at a high temperature rise rate, and combining an appropriate proportion of organic phosphorus compounds to suppress outgassing and increase the density of the graphite layer.

Benefits of technology

Achieved thick graphite sheets with good productivity at high heating rates, high density and excellent thermal conductivity, avoiding surface foaming problems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005005072510000271
    Figure BDA0005005072510000271
Patent Text Reader

Abstract

The present invention addresses the problem of providing a polyimide film with which it is possible to provide graphite flakes having high density with good productivity. The aforementioned problem is solved by a polyimide film for a graphite sheet, which is a polyimide film that uses an acid dianhydride component and a diamine component as raw materials, and which is characterized in that the total content of BTDA, ODPA, and BAPP is 1-50 mol% or less with respect to the total amount of 200 mol% of the acid dianhydride component and the diamine component, and the total content of BTDA, ODPA, and BAPP is 1-50 mol% or less with respect to the total amount of 200 mol% of the diamine component. And the polyimide film for the graphite sheet contains a predetermined amount of an organic phosphorus compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyimide film for a graphite sheet, a graphite sheet and a method for producing the same. Background Art

[0002] Graphite sheets have excellent thermal conductivity and are therefore used as heat dissipating members in various electronic devices such as computers, semiconductor elements and other heat-generating components mounted in electrical equipment, and the like.

[0003] As a method for producing such a graphite sheet, for example, Patent Documents 1 to 3 describe techniques for producing a graphite sheet by heat-treating (graphitizing) a polyimide film.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Publication No. 2003-165714

[0007] Patent Document 2: Japanese Patent Publication No. 2016-17169

[0008] Patent Document 3: Japanese Patent Publication No. 2020-164611

[0009] Patent Document 4: Japanese Patent Publication No. 2014-136721 Summary of the invention

[0010] Problem that the invention aims to solve

[0011] However, the above-mentioned technology has problems regarding the density and productivity of the obtained graphite sheet.

[0012] An object of one embodiment of the present invention is to provide a polyimide film capable of providing a high-density graphite sheet with good productivity.

[0013] Solutions for solving problems

[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems and have completed the present invention.

[0015] That is, one embodiment of the present invention includes the following.

[0016] A polyimide film for a graphite sheet, which is a polyimide film made of an acid dianhydride component and a diamine component.

[0017] The acid dianhydride component contains 50 to 100 mol% of pyromellitic dianhydride (PMDA) and 0 to 50 mol% of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in the total amount of 100 mol% of the acid dianhydride component, and the diamine component contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA), 2,2-bis[4-(4-aminophenoxy)phenyl]propanediol in the total amount of 100 mol% of the diamine component. The polyimide film contains 0.1 to 5.0 wt % of the organic phosphorus compound in the total amount of 100 wt % of the polyimide film.

[0018] A method for producing a polyimide film, comprising: a step of mixing an acid dianhydride component and a diamine component to obtain a polyamic acid; and a step of adding 0.1 to 5.0 weight percent of an organic phosphorus compound to 100 weight percent of the polyamic acid, wherein the acid dianhydride component contains 50 to 100 mole percent of pyromellitic dianhydride (PMDA), 0 to 50 mole percent of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mole percent of the total amount of the acid dianhydride component, and the diamine component contains 0.1 to 5.0 weight percent of an organic phosphorus compound in 100 weight percent of the total amount of the acid dianhydride component. The total amount of the amine component (100 mol%) contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP). The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to the total amount of the acid dianhydride component and the diamine component (200 mol%).

[0019] A method for producing a graphite sheet, comprising a step of heat-treating a polyimide film for a graphite sheet at a temperature of 2400° C. or higher, wherein the polyimide film for a graphite sheet is a polyimide film made of an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA) and 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mol % of the total amount of the acid dianhydride components, and the diamine component contains 4,4'-diaminodiphenylamine in 100 mol % of the total amount of the diamine components. 50 to 100 mol% of phenyl ether (ODA), 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), with respect to the total amount of the aforementioned acid dianhydride component and the aforementioned diamine component of 200 mol%, the total content of the aforementioned 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the aforementioned 4,4'-oxydiphthalic dianhydride (ODPA) and the aforementioned 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol%, and the polyimide film contains 0.1 to 5.0 wt% of the organic phosphorus compound in 100 wt% of the total amount of the aforementioned polyimide film.

[0020] Effects of the Invention

[0021] According to one embodiment of the present invention, it is possible to provide a polyimide film capable of providing a high-density graphite sheet with good productivity. DETAILED DESCRIPTION

[0022] An embodiment of the present invention is described below, but the present invention is not limited thereto. The present invention is not limited to the various structures described below, and various changes can be made within the scope shown in the claims. The embodiments or embodiments obtained by appropriately combining the technical means disclosed in different embodiments or embodiments are also included in the technical scope of the present invention. In addition, all academic documents and patent documents recorded in this specification are cited in this specification as references. In addition, unless otherwise specified in this specification, "A to B" indicating a numerical range means "above A and below B".

[0023] <1. Technical concept of the present invention>

[0024] In recent years, as electronic devices have become more high-performance, thick graphite sheets (thick graphite sheets) with better heat dissipation performance are required. Thick graphite sheets can be produced by heat treating (graphitizing) a thick polyimide film (for example, 80 μm or more). However, the present inventors have found that, for conventional polyimide films, when the thickness is simply increased, the graphite sheet containing the polyimide film as a raw material (after heat treatment) will have problems such as large foaming on the surface of the graphite sheet and reduced thermal conductivity, resulting in poor appearance.

[0025] As a cause of the problems occurring in such a thick graphite sheet, the present inventors have focused on outgassing generated in the graphite sheet when a polyimide film is heat-treated.

[0026] In the past, in the case of manufacturing thinner graphite sheets, acid anhydrides (PMDA, BPDA, etc.) and / or diamines (ODA, PDA, etc.) were used as raw materials for polyimide films for the purpose of improving interlayer strength, etc., which have the effect of improving the orientation of polyimide films, that is, the effect of improving the orientation of graphite (graphite layer) in the obtained graphite sheets. However, in thick graphite sheets, since the number of graphite layers increases, when the aforementioned acid anhydrides and / or diamines that have the effect of improving the orientation of polyimide films are used as raw materials for polyimide films, the exhaust gas generated in the graphite sheet (between the graphite layers) due to the heat treatment of the polyimide film is blocked by the majority of graphite layers with high orientation, and is not discharged from the inside of the graphite sheet, but is filled in the interlayers of the graphite layers. Moreover, as the heating progresses, the amount of the exhaust gas increases, and the volume of the exhaust gas increases, thereby squeezing the surface of the graphite layer. It is considered that the squeezing of the graphite layer caused by the exhaust gas is the main cause of problems such as foaming (bulging) on ​​the surface of the graphite sheet.

[0027] When a polyimide film is heat-treated, in order to suppress the generation of outgassing, it is necessary to reduce the heating rate during the heat treatment (for example, to less than 0.1°C / min). That is, for conventional polyimide films, in order to suppress the generation of problems caused by outgassing, it is necessary to reduce the heating rate to a level that can suppress the generation of outgassing. However, when the heating rate is reduced to a level that can suppress the generation of outgassing, the time required for the heat treatment of the polyimide film increases, and the productivity of the graphite sheet is greatly reduced. That is, conventional polyimide films have the problem of greatly reducing the productivity of the graphite sheet when manufacturing thick graphite sheets.

[0028] In addition, as electronic devices have become smaller in recent years, graphite sheets are required to have a high density in order to achieve efficient heat dissipation in order to be placed in limited space within the small electronic devices.

[0029] In view of such a situation, the present inventors have conducted intensive studies to provide a polyimide film that can provide a high-density graphite sheet with good productivity, and in particular, a polyimide film that can provide a high-density graphite sheet with good productivity even when the polyimide film is thick enough to provide a thick graphite sheet. As a result, the present inventors have found the following findings and have completed the present invention.

[0030] (1) By using an appropriate amount of anhydrides (BTDA, ODPA, etc.) and / or diamines (BAPP, etc.) that have the effect of disturbing (reducing) the orientation of the polyimide film as the raw material of the polyimide film, the orientation of the obtained polyimide film can be disturbed appropriately. Moreover, when the polyimide film with such moderately disturbed orientation is subjected to heat treatment, the orientation of the graphite layer in the obtained graphite sheet can be disturbed appropriately. Moreover, by moderately disturbing the orientation of the graphite layer in the graphite sheet, the exhaust gas generated in the graphite sheet can be removed appropriately. Therefore, even when the polyimide film is heat treated at a high temperature rise rate, problems such as bubbling on the surface of the graphite sheet caused by the exhaust gas will not occur, so that the graphite sheet can be provided with good productivity;

[0031] (2) By heat-treating a polyimide film containing an organic phosphorus compound in an appropriate proportion, a graphite sheet having a high density can be provided.

[0032] The polyimide film of one embodiment of the present invention contains an appropriate amount of anhydride and / or diamine that has the effect of disturbing the orientation of the polyimide film, and contains an appropriate proportion of an organic phosphorus compound, so that a high-density graphite sheet can be provided with good productivity. Therefore, it can be appropriately used for the production of graphite sheets, especially thick graphite sheets. Such a polyimide film is previously unknown and can be said to be a surprising discovery.

[0033] <2. Polyimide film>

[0034] Hereinafter, a polyimide film according to an embodiment of the present invention (hereinafter, sometimes referred to as the present polyimide film) is described in detail. The present polyimide film is a polyimide film made of an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol% of PMDA, 0 to 50 mol% of at least one of BTDA and ODPA in 100 mol% of the total amount of the acid dianhydride component, and the diamine component contains 50 to 100 mol% of ODA and 0 to 50 mol% of BAPP in 100 mol% of the total amount of the diamine component, and the total content of the BTDA, the ODPA and the BAPP is 1 to 50 mol% or less relative to the total amount of the acid dianhydride component and the diamine component, which is 200 mol%, and the polyimide film contains 0.1 wt% to 5.0 wt% of an organic phosphorus compound.

[0035] The polyimide film has the above-mentioned structure, so by using the polyimide film as a raw material, a high-density graphite sheet can be provided with good productivity. That is, the polyimide film can be appropriately used for the manufacture of a graphite sheet. Therefore, the polyimide film can also be called a polyimide film for a graphite sheet.

[0036] (Acid dianhydride component)

[0037] The acid dianhydride component as the raw material of the present polyimide film includes 50 to 100 mol% of pyromellitic dianhydride (PMDA), and includes 0 to 50 mol% of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA). The acid dianhydride component may include any one of BTDA and ODPA, or may include two. In addition, when the present polyimide film uses 1 mol% or more of BAPP as a raw material as the diamine component described later, the acid dianhydride component may include BTDA and / or ODPA, or may not include BTDA and ODPA.

[0038] In one embodiment of the present invention, the amount of PMDA contained in the acid dianhydride component is 50 mol% or more relative to the total amount of the acid dianhydride component 100 mol%, preferably 60 mol% or more, more preferably 70 mol% or more. By making the polyimide film contain more than 50 mol% of PMDA, a polyimide film (and carbonaceous film) with appropriate orientation can be provided. The amount of PMDA contained in the acid dianhydride component can be 80 mol% or more, 90 mol% or more, 95 mol% or more, or 100 mol%.

[0039] The acid dianhydride component preferably contains 100 mol% of PMDA, in which case the diamine component preferably contains 50 to 99 mol% of ODA and 1 to 50 mol% of BAPP. With such a configuration, the obtained graphite sheet has good thermal diffusivity and flexibility.

[0040] In one embodiment of the present invention, when the acid dianhydride component includes at least one of BTDA and ODPA, the content of BTDA and ODPA (the total amount of BTDA and ODPA) relative to the total amount of 100 mol% of the acid dianhydride component is 1 mol% or more, preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 20 mol% or more. The upper limit of the content of BTDA and ODPA is 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less. When the acid dianhydride component includes at least one of BTDA and ODPA 1 mol% or more, the orientation of the obtained polyimide film (and carbonaceous film) can be appropriately disturbed. Thus, a graphite sheet can be provided with good productivity. In addition, when the content (total amount) of at least one of BTDA and ODPA in the acid dianhydride component is 50 mol% or less, there is no worry about excessively disturbing the orientation of the obtained graphite sheet, and the thermal diffusivity and flexibility of the obtained graphite sheet are good. In other words, when the content (total amount) of BTDA and ODPA exceeds 50 mol %, the orientation of the graphite layers in the obtained graphite sheet is excessively disturbed, and the thermal conductivity and flexibility of the graphite sheet tend to be poor.

[0041] The polyimide film may contain other acid dianhydrides as acid dianhydride components in addition to the aforementioned PMDA, the aforementioned BTDA and the aforementioned ODPA. Examples of other acid dianhydrides include 2,3,6,7-naphthalenetetracarboxylic dianhydride, 1,2,5,6-naphthalenetetracarboxylic dianhydride, 2,2',3,3'-biphenyltetracarboxylic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 3,4,9,10-perylenetetracarboxylic dianhydride, 1,1-(3,4-dicarboxyphenyl)ethane ...2 1-bis(2,3-dicarboxyphenyl)ethane dianhydride, 1,1-bis(3,4-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, p-phenylene bis(trimellitic acid monoester dianhydride), ethylene bis(trimellitic acid monoester dianhydride), bisphenol A bis(trimellitic acid monoester dianhydride), and the like. As other acid dianhydrides, these acid dianhydrides may be used alone or in combination of a plurality of these acid dianhydrides in any ratio.

[0042] The content of the aforementioned other acid dianhydrides in the acid dianhydride component as the raw material of the present polyimide film is 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less, further preferably 20 mol% or less, further preferably 10 mol% or less, and particularly preferably 0 mol% in the total amount 100 mol% of the aforementioned acid dianhydride component. That is, the acid dianhydride component as the raw material of the present polyimide film particularly preferably does not contain other acid dianhydrides.

[0043] (Diamine component)

[0044] The diamine component as a raw material of the present polyimide film contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP). When the present polyimide film uses 1 mol% or more of BTDA or ODPA as a raw material as the acid dianhydride component, the diamine component may or may not contain BAPP.

[0045] In one embodiment of the present invention, the amount of ODA contained in the diamine component is 50 mol% or more relative to the total amount of the diamine component 100 mol%, preferably 60 mol% or more, more preferably 70 mol% or more. By making the polyimide film contain ODA 50 mol% or more, it is possible to provide a polyimide film (and carbonaceous film) with appropriate orientation. The amount of ODA contained in the diamine component can be 80 mol% or more, 90 mol% or more, 95 mol% or more, or 100 mol%.

[0046] The diamine component preferably contains 100 mol% of ODA, and in this case, the acid dianhydride component preferably contains 50 to 99 mol% of PMDA and 1 to 50 mol% of at least one of BTDA and ODPA. With such a configuration, the obtained graphite sheet has good thermal diffusivity and flexibility.

[0047] In one embodiment of the present invention, when the diamine component contains BAPP, the content of BAPP is 1 mol% or more relative to the total amount of the diamine component 100 mol%, preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 20 mol% or more. The upper limit of the content of BAPP is 50 mol% or less, preferably 40 mol% or less, and more preferably 30 mol% or less. When the diamine component contains 1 mol% or more of BAPP, the orientation of the obtained polyimide film (and carbonaceous film) can be appropriately disturbed. Thus, a graphite sheet can be provided with good productivity. In addition, when the content of BAPP in the diamine component is 50 mol% or less, there is no worry about excessively disturbing the orientation of the graphite layer in the graphite sheet, and the thermal diffusivity and flexibility of the obtained graphite sheet are good.

[0048] The polyimide film may contain other diamines as diamine components in addition to the aforementioned ODA and BAPP. Examples of other diamines include p-phenylenediamine (PDA), 4,4'-diaminodiphenylmethane, benzidine, 3,3'-dichlorobenzidine, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 1,5-diaminonaphthalene, 4,4'-diaminodiphenyldiethylsilane, 4,4'-diaminodiphenylsilane, 4,4'-diaminodiphenylethylphosphine oxide, 4,4'-diaminodiphenyl N-methylamine, 4,4'-diaminodiphenyl N-phenylamine, 1,3-diaminobenzene, 1,2-diaminobenzene, and analogs thereof. As other diamines, these diamines may be used alone or in combination of two or more thereof in any proportion.

[0049] The content of the aforementioned other diamine in the diamine component as a raw material of the present polyimide film is 50 mol% or less, preferably 40 mol% or less, more preferably 30 mol% or less, further preferably 20 mol% or less, further preferably 10 mol% or less, and particularly preferably 0 mol% in the total amount 100 mol% of the aforementioned diamine component. That is, the diamine component as a raw material of the present polyimide film particularly preferably does not contain other diamines.

[0050] (Total content of BTDA, ODPA and BAPP)

[0051] The polyimide film contains 1 to 50 mol% of the BTDA, ODPA and BAPP relative to the total amount of 200 mol% of the acid dianhydride component and the diamine component. By making the amount of the BTDA, ODPA and BAPP in the polyimide film within the above range, the orientation of the polyimide film (and the carbonaceous film) can be appropriately disturbed. Therefore, the graphite sheet containing the polyimide film as a raw material is a graphite sheet with good productivity that can be produced at a high heating rate.

[0052] In the present polyimide film, the lower limit of the total content of the BTDA, ODPA and BAPP relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component is 1 mol% or more, preferably 5 mol% or more, more preferably 10 mol% or more, and further preferably 20 mol% or more. In addition, the upper limit of the total content of the BTDA, ODPA and BAPP is 50 mol% or less, preferably 40 mol% or less, and more preferably 30 mol% or less.

[0053] The polyimide film is a polyimide film made of substantially equimolar amounts of the above-mentioned acid dianhydride component and the above-mentioned diamine component. It should be noted that, in this specification, substantially equimolar amounts means that the ratio of the molar amounts of two or more different substances (for example, the acid dianhydride component and the diamine component) is within the range of 100:98 to 100:102, preferably 100:100. That is, in this specification, "100 mol% of the total amount of the acid dianhydride component contains 0 to 50 mol% of at least one of BTDA and ODPA" can also be said to be "relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component, 0 to 50 mol% of at least one of BTDA and ODPA is contained", and "100 mol% of the total amount of the diamine component contains 0 to 50 mol% of BAPP" can also be said to be "relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component, 0 to 50 mol% of BAPP is contained". That is, "the total content of the BTDA, ODPA and BAPP relative to 200 mol % of the total amount of the acid dianhydride component and the diamine component" can be calculated as the total content of BTDA and ODPA in the acid dianhydride component and the content of BAPP in the diamine component.

[0054] (Organophosphorus compounds)

[0055] The polyimide film of the present invention contains 0.1 to 5.0 wt % of an organic phosphorus compound based on 100 wt % of the total amount of the polyimide film.

[0056] The content of the organic phosphorus compound in the polyimide film is 0.1 to 5.0% by weight, preferably 0.2 to 3.0% by weight, and more preferably 0.3 to 1.5% by weight, based on 100% by weight of the total amount of the polyimide film. When the content of the organic phosphorus compound in the polyimide film is 0.1% by weight or more, a high-density graphite sheet can be provided, and when the content of the organic phosphorus compound in the polyimide film is 5.0% by weight or less, there is an advantage that the foaming rate during graphitization is reduced, and a graphite sheet can be provided with better productivity. In addition, the polyimide film contains the organic phosphorus compound in the above range, which also has the following advantages: (1) a graphite sheet with excellent peelability from a micro-adhesive film can be provided, and (2) the carbonaceous film can be prevented from fusing in the graphitization process, so that a graphite sheet can be provided with better productivity.

[0057] As the organophosphorus compounds that can be contained in the polyimide film, phosphates, phosphine oxides, phosphites, phosphines, phosphonates, phosphinates, etc. can be cited. Only one of these organophosphorus compounds can be contained, or two or more can be contained. Among the organophosphorus compounds exemplified, phosphates are preferred, and triphenyl phosphate is particularly preferred, because they have the advantage of being stable in the air.

[0058] From the viewpoint of stability, the organic phosphorus compound contained in the polyimide film is preferably an organic phosphorus compound having a valence of phosphorus of 5. That is, the polyimide film preferably contains an organic phosphorus compound having a valence of phosphorus of 5 as the organic phosphorus compound, and more preferably contains only an organic phosphorus compound having a valence of phosphorus of 5.

[0059] Examples of the organic phosphorus compound having a phosphorus valence of five include triphenyl phosphate and trimethyl phosphate.

[0060] The organophosphorus compound that may be included in the polyimide film has a weight loss rate of 5% at a temperature of preferably 200° C. or higher, more preferably 250° C. or higher, and further preferably 300° C. or higher. When the organophosphorus compound included in the polyimide film has a weight loss rate of 5% at a temperature of 200° C. or higher, the contamination of the furnace for manufacturing the polyimide film can be reduced.

[0061] Examples of the organic phosphorus compound at which the temperature at which the weight loss rate reaches 5% in the TG-DTA measurement is 200° C. or higher include triphenyl phosphate and triphenylphosphine oxide.

[0062] (Inorganic particles)

[0063] The polyimide film may contain inorganic particles (filler). When the polyimide film contains inorganic particles, the polyimide film is a polyimide film with excellent sliding properties. Such a polyimide film with excellent sliding properties can suppress the generation of damage during the transportation of the polyimide film, and can also prevent the welding of the carbonaceous film in the graphitization process.

[0064] Examples of inorganic particles that may be contained in the polyimide film include calcium carbonate (CACO3), silicon dioxide, calcium hydrogen phosphate (CAHPO4), calcium phosphate (CA2P2O7), etc. Among these inorganic particles, inorganic particles containing phosphorus such as calcium hydrogen phosphate and calcium phosphate are preferred.

[0065] The upper limit of the average particle size of the inorganic particles that the polyimide film may contain is not particularly limited, and is preferably 2.5 μm or less, preferably 2.0 μm or less, preferably 1.5 μm or less, and preferably 1.0 μm or less. When the average particle size of the inorganic particles is 2.5 μm or less, the voids generated inside the film after graphitization can be reduced, and a graphite sheet with excellent density can be obtained after compression. In particular, by being 1.0 μm or less, a graphite sheet with even better density can be provided. In addition, the lower limit of the average particle size of the inorganic particles is not particularly limited, and is preferably 0.1 μm or more, more preferably 0.3 μm or more, further preferably 0.5 μm or more, and further more preferably 0.7 μm or more.

[0066] In addition, in this specification, the average particle diameter of inorganic particles refers to a volume average particle diameter, which is a value measured using a particle size distribution measuring apparatus MT3000II manufactured by MicrotrAc Co., Ltd. for inorganic particles dispersed in dimethylformamide.

[0067] When the polyimide film contains inorganic particles, the lower limit of the content of the inorganic particles in the polyimide film is not particularly limited, preferably 0.01% by weight or more, more preferably 0.02% by weight, and further preferably 0.03% by weight or more. The upper limit of the content of the inorganic particles is not particularly limited, preferably 0.30% by weight or less, more preferably 0.20% by weight or less, further preferably 0.15% by weight or less, and further more preferably 0.10% by weight or less.

[0068] (Thickness of polyimide film)

[0069] The thickness of the polyimide film is preferably 80 μm to 200 μm, more preferably more than 80 μm and 200 μm or less, further preferably 90 μm to 180 μm, further preferably 100 μm to 170 μm, particularly preferably 110 μm to 150 μm, and most preferably 115 μm to 140 μm. When the thickness of the polyimide film is within the above range, a graphite sheet with a better thermal diffusivity can be provided.

[0070] The lower limit of the thickness of the polyimide film of one embodiment of the present invention is preferably 80 μm or more, more preferably more than 80 μm, further preferably 90 μm or more, further preferably 100 μm or more, particularly preferably 110 μm or more, and most preferably 115 μm or more. In addition, the upper limit of the thickness of the polyimide film is preferably 200 μm or less, more preferably 180 μm or less, further preferably 160 μm or less, further preferably 140 μm or less, and particularly preferably 150 μm or less. A polyimide film having a thickness of 80 μm or more can be said to be a polyimide film with a large thickness, and can also be said to be a polyimide film that can provide a thick graphite sheet.

[0071] Conventional polyimide films have problems such as poor productivity of the obtained graphite sheet when the thickness of the polyimide film is increased (e.g., a thickness of 80 μm or more) in order to provide a thick graphite sheet. However, the present polyimide film can provide a thick graphite sheet with good productivity even when it is made into a thick polyimide film, and further, the obtained graphite sheet has a high density. That is, the present polyimide film can be suitably used as a thick polyimide film.

[0072] <3. Method for producing polyimide film>

[0073] The method for producing a polyimide film according to one embodiment of the present invention (hereinafter, sometimes referred to as the method for producing the present polyimide film) is not particularly limited, and for example, a method having the following steps i) to iv) is preferred;

[0074] i) a step of reacting an acid dianhydride component with a diamine component in an organic solvent to obtain a polyamic acid solution;

[0075] ii) coating the polyamic acid solution on a support to form a mixed solution layer;

[0076] iii) drying (heating) the mixed solution layer on the support to form a self-supporting gel film, and then peeling the gel film from the support;

[0077] iv) A step of further heating the peeled gel film to imidize the remaining amic acid and drying the gel film to obtain a polyimide film.

[0078] The acid dianhydride component and the diamine component can also be said to be monomer units constituting the polyamic acid, which is a copolymer. In this specification, the acid dianhydride component and the diamine component may be collectively referred to as a monomer component.

[0079] The step i) in the method for producing the polyimide film is not particularly limited as long as the acid dianhydride component and the diamine component described in detail in the aforementioned item <2. Polyimide film> can be polymerized (as raw materials) to obtain polyamic acid. For example, any of the following polymerization methods (1) to (5) can be appropriately used.

[0080] (1) A method of dissolving a diamine component in an organic solvent (organic polar solvent) and reacting the diamine component with an acid dianhydride component in a substantially equimolar amount thereof to perform polymerization.

[0081] (2) A method in which an acid dianhydride component and a diamine component in a molar amount smaller than the acid dianhydride component are reacted in an organic solvent to obtain a prepolymer having acid dianhydride groups at both ends. Subsequently, the diamine component is polymerized with the prepolymer in such a manner that the total amount used in the entire polymerization step is substantially equimolar to the acid dianhydride component.

[0082] A specific example of the method (2) is as follows: a prepolymer having the acid dianhydride at both ends is synthesized using a diamine component and an acid dianhydride component, and the prepolymer is reacted with a diamine component having the same composition as the diamine component used in the synthesis of the prepolymer or a diamine component having a different composition to synthesize a polyamic acid. In the method (2), the diamine component reacting with the prepolymer may be a diamine component having the same composition as the diamine component used in the synthesis of the prepolymer or a diamine component having a different composition.

[0083] (3) A method of reacting an acid dianhydride component with a diamine component in excess molar amount relative to the acid dianhydride component in an organic solvent to obtain a prepolymer having amino groups at both ends. Then, after adding a diamine component to the prepolymer, the acid dianhydride component is added in such a manner that the total amount of the acid dianhydride component and the diamine component used in the entire polymerization step is substantially equimolar, and the prepolymer and the acid dianhydride component are polymerized.

[0084] (4) A method of polymerizing an acid dianhydride component with a diamine component by dissolving and / or dispersing the acid dianhydride component in an organic solvent and then adding the diamine component in a substantially equimolar amount relative to the acid dianhydride component.

[0085] (5) A method of polymerizing by reacting a mixture of substantially equimolar amounts of an acid dianhydride component and a diamine component in an organic solvent.

[0086] i) The process preferably includes an addition process of further adding (mixing) an organic phosphorus compound to the polyamic acid solution obtained by polymerizing the acid dianhydride component and the diamine component. The amount of the organic phosphorus compound added relative to the solid content (polyamic acid) of the polyamic acid solution in the addition process is the content of the organic phosphorus compound in the obtained polyimide film. In other words, the content of the organic phosphorus compound in the obtained polyimide film can be adjusted by adjusting the amount of the organic phosphorus compound added in the addition process.

[0087] The acid dianhydride component and the diamine component that react (are provided for polymerization) in the step i) are the acid dianhydride component and the diamine component that are the raw materials of the obtained polyimide film. In addition, the amount of the organic phosphorus compound added relative to the polyamic acid in the step i) (addition step) can be the content of the organic phosphorus compound in the obtained polyimide film. Therefore, the step i) in the method for producing the polyimide film can be described as follows: it includes a step of mixing the acid dianhydride component and the diamine component to obtain polyamic acid; and a step of adding 0.1 to 5.0 weight % of the organic phosphorus compound to 100 weight % of the above-mentioned polyamic acid, wherein the above-mentioned acid dianhydride component contains 50 to 100 mol % of pyromellitic anhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic anhydride (BTDA) and 4,4'-oxydiphthalic anhydride (ODPA) in 100 mol % of the total amount of the above-mentioned acid dianhydride component. The amine component contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in 100 mol% of the total amount of the diamine component. The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component.

[0088] In addition, a preferred method for producing the polyimide film can be described as follows: a method comprising: a step of mixing an acid dianhydride component and a diamine component to obtain a polyamic acid; and a step of adding 0.1 to 5.0 weight % of an organic phosphorus compound to 100 weight % of the polyamic acid, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mol % of the total amount of the acid dianhydride component. The diamine component contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in 100 mol% of the total amount of the diamine component. The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component.

[0089] Regarding the acid dianhydride component and diamine component reacted (subjected to polymerization) in step i) in the present method for producing a polyimide film, and the organic phosphorus compound added to the polyamic acid, the description in the above section <2. Polyimide film> can be appropriately cited.

[0090] The steps ii) to iv) in the method for producing the polyimide film can also be said to be steps for imidizing the aforementioned polyamic acid solution to obtain the polyimide film. In the steps ii) to iv), as the method for imidizing the polyamic acid, for example, the following methods can be used: (I) a thermal imidization method in which the polyamic acid solution is heated without using an imidization accelerator to imidize the polyamic acid solution; or (II) a chemical imidization method in which an imidization accelerator such as a dehydrating agent (dehydration ring-closing agent) represented by an acid dianhydride such as acetic anhydride and / or a catalyst represented by a tertiary amine such as picoline, quinoline, isoquinoline, pyridine, etc. is added to the polyamic acid, and the polyamic acid solution containing the imidization accelerator is heated to imidize the polyamic acid.

[0091] In particular, the chemical imidization method is preferred from the viewpoint that the linear expansion coefficient of the obtained polyimide film is small, the elastic modulus is high, the birefringence is easy to increase, and rapid graphitization can be achieved at a relatively low temperature, and a graphite sheet of good quality can be obtained. In particular, by using a dehydrating agent and an imidization accelerator in combination, the linear expansion coefficient of the obtained polyimide film is smaller, the elastic modulus is larger, and the birefringence can be larger, so it is preferred. In addition, the chemical imidization method is an industrially advantageous method with excellent productivity because the imidization reaction is carried out more rapidly, so the imidization reaction can be completed in a short time during the heat treatment.

[0092] In the method for producing the polyimide film, the support used in step ii) is not particularly limited as long as it is a support that is not dissolved by the solution containing the aforementioned polyimide and can withstand the heating required for drying the aforementioned laminate. For example, a glass plate, aluminum foil, an endless stainless steel belt, a stainless steel drum, etc. can be appropriately used.

[0093] More specifically, step iii) is a step in which the heating conditions are set according to the thickness and production rate of the final polyimide film, the mixed solution layer (polyamic acid solution) coated on the support is partially imidized or dried, and then the gel film is obtained (peeled off) from the support.

[0094] More specifically, the step iv) is a step of fixing the end of the aforementioned gel film (the gel film obtained in the aforementioned step iii) and subjecting it to heat treatment while avoiding shrinkage during curing, thereby removing water, residual solvent, imidization accelerator, etc. from the aforementioned gel film and completely imidizing the remaining amic acid (unimidized amic acid) to obtain a film containing polyimide (polyimide film). The heating conditions in the step iv) can be appropriately set according to the thickness of the film to be finally obtained and the production speed.

[0095] In addition, the drying method of the mixed solution layer and the gel film in the steps iii) and iv) is not particularly limited, and for example, a method of heating by hot air treatment using a hot air oven or the like and / or a method of heating by radiant heat ray treatment using a far infrared heater or the like can be cited. The drying temperature (heating temperature) in the drying step is not particularly limited as long as a gel film or a polyimide film can be obtained, and for example, it can be 100° C. to 140° C. in the case of hot air treatment, and can be 400° C. to 500° C. in the case of using an infrared heater.

[0096] <4. Graphite sheet>

[0097] In one embodiment of the present invention, a graphite sheet is provided, which contains the present polyimide film as a raw material. The graphite sheet of one embodiment of the present invention (hereinafter referred to as the present graphite sheet) can also be said to be a graphite sheet formed by heat treating the present polyimide film. The present graphite sheet contains the present polyimide film as a raw material, so it has a high density and can be provided with good productivity. It should be noted that in this specification, the present graphite sheet refers to both the graphite sheet before the calendering process described later (graphite sheet before calendering) and the graphite sheet after the calendering process (graphite sheet after calendering). If there is no special explanation, it refers to the graphite sheet after calendering.

[0098] The density of the graphite sheet (graphite sheet after rolling) is preferably more than 2.00 g / cm 3 , more preferably 2.02 g / cm 3 More preferably, 2.04 g / cm 3 More preferably, it is 2.06 g / cm 3 The upper limit of density is not particularly limited, but the density of graphite sheets is usually 2.26 g / cm 3 Below. Density is 2.00g / cm 3 The above graphite sheet can be said to be a high-density graphite sheet that can achieve efficient heat dissipation and can be suitably used as a heat dissipation member in fields requiring excellent heat dissipation such as electronic equipment. It should be noted that the method for measuring the density of the graphite sheet is described in the examples described below.

[0099] (Thermal conductivity)

[0100] In this specification, the thermal conductivity of a graphite sheet can be evaluated by the thermal diffusivity of the graphite sheet (rolled graphite sheet). The thermal diffusivity of the graphite sheet is preferably 7.0 cm 2 / s or more, more preferably 8.0 cm 2 / s or more, more preferably 9.0m 2 / s or more, more preferably 9.5 cm 2 / s or more. Thermal diffusivity is 7.0cm 2 The graphite sheet having a thermal conductivity of 1000 nm or more has excellent thermal conductivity. In other words, it has excellent heat dissipation and can be suitably used as a heat dissipation component in fields requiring excellent heat dissipation, such as electronic equipment. It should be noted that the method for measuring the thermal diffusivity of the graphite sheet is described in the examples described below.

[0101] (productivity)

[0102] In this specification, the productivity of the graphite sheet can be evaluated based on the ratio of the thickness of the polyimide film as a raw material to the thickness of the obtained graphite sheet (graphite sheet before calendering) (thickness of the graphite sheet before calendering / thickness of the polyimide film, hereinafter referred to as "GS thickness / PI thickness"). When the GS thickness / PI thickness is greater than a certain value (for example, more than 3.0), the graphite sheet refers to a graphite sheet with poor productivity that is substantially unable to be heat treated at a high heating rate due to foaming on the surface during heat treatment. On the other hand, it means that the smaller the GS thickness / PI thickness, the more the foaming caused by the exhaust during the heat treatment of the graphite sheet is suppressed, and it can be said that it is a graphite sheet with excellent productivity that can be heat treated at a high heating rate. Specifically, when the GS thickness / PI thickness is less than 3.0, it can be evaluated that the productivity of the graphite sheet is excellent. The GS thickness / PI thickness is preferably less than 2.5, more preferably less than 2.0, further preferably less than 1.5, and further preferably less than 1.0.

[0103] The lower limit of the thickness of the graphite sheet (calendered graphite sheet) is preferably 45 μm or more, more preferably 50 μm or more, and further preferably 55 μm or more. In addition, the upper limit of the thickness of the graphite sheet after calendering is preferably 110 μm or less, and more preferably 105 μm or less. When the thickness of the graphite sheet after calendering is 45 μm or more, the graphite sheet can be said to be a graphite sheet with sufficient thickness, which can achieve efficient heat dissipation. In addition, when the thickness is 110 μm or less, it has the advantage of being able to be mounted in thin electronic devices with little extra space.

[0104] <5. Method for producing graphite sheet>

[0105] A method for producing a graphite sheet according to an embodiment of the present invention (hereinafter sometimes referred to as the method for producing the present graphite sheet) is not particularly limited as long as the present graphite sheet, i.e., a graphite sheet with high density, can be provided with good productivity, and is a method comprising the step of heat-treating a polyimide film for a graphite sheet at 2400° C. or higher, wherein the polyimide film for a graphite sheet is a polyimide film made of an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mol % of the total amount of the acid dianhydride component, and wherein the polyimide film is a polyimide film having an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA), and wherein the polyimide film is a polyimide film having an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 0 to 50 mol % of at least any one of ... The diamine component contains 50 to 100 mol% of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) in 100 mol% of the total amount of the diamine component, the total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component, and the polyimide film contains 0.1 to 5.0 wt% of the organic phosphorus compound in 100 wt% of the total amount of the polyimide film. The method for producing the graphite sheet can also be said to be a method including a step of heat-treating the polyimide film at 2400°C or higher.

[0106] According to the method for producing a graphite sheet, a high-density graphite sheet can be provided with good productivity.

[0107] The method for producing the graphite sheet is described in detail below, taking as an example a method including a step of heat treating a specific polyimide film at 2400° C. or higher. In the following description, the description in the above section <2. Polyimide film> is appropriately cited for specific aspects of the polyimide film.

[0108] The method for manufacturing the present graphite sheet is not particularly limited as long as it includes a process of heat-treating a specific polyimide film (the present polyimide film) at a temperature of 2400°C or above, and is preferably a so-called polymer thermal decomposition method in which the polyimide film is heat-treated under an inert gas atmosphere and reduced pressure. Specifically, the method for manufacturing the present graphite sheet is preferably a method including the following steps: a carbonization step of preheating the polyimide film at a temperature of about 1000°C to obtain a carbonized polyimide film; a graphitization step of heat-treating (heating) the carbonized polyimide film produced by the carbonization step at a temperature of 2400°C or above to graphitize it; and a calendering step of calendering it. It should be noted that in the method for manufacturing the present graphite sheet, the carbonization step and the graphitization step can be performed continuously, or the graphitization step can be performed separately after the carbonization step is completed.

[0109] Hereinafter, the carbonization step, graphitization step, and calendering step that may be included in the method for producing the graphite sheet will be described in detail.

[0110] (Carbonization process)

[0111] The carbonization process is a process of heat-treating the polyimide film at a temperature of about 1000°C to carbonize the polyimide film (carbonization). The carbonization method of the polyimide film in the carbonization process is not particularly limited. For example, a rectangular polyimide film can be carbonized in a state stacked with a graphite sheet, a rolled polyimide film can be carbonized in a rolled state, or a film can be released from the rolled polyimide film and continuously carbonized. The carbonization process is preferably carried out in a vacuum atmosphere, under reduced pressure or in an inert gas. As an inert gas, nitrogen can be appropriately used. It should be noted that in this specification, the carbonized polyimide film obtained by the carbonization process is sometimes referred to as a carbonaceous film.

[0112] (Graphitization process)

[0113] The graphitization process is a process of heat-treating the carbonaceous film obtained in the carbonization process at a temperature of 2400°C or more to graphitize the carbonaceous film. The graphitization process can also be said to be a process of heat-treating the carbonaceous film to obtain a graphite sheet (graphite sheet before rolling). In the graphitization process, as the temperature (maximum temperature) when the carbonaceous film obtained in the carbonization process is heat-treated, for example, it is preferably above 2400°C, above 2600°C, above 2800°C, above 2900°C, or above 3000°C. The upper limit of the maximum temperature is not particularly limited, preferably below 3300°C, and more preferably below 3200°C. In the graphitization process, when the temperature (maximum temperature) when the carbonaceous film obtained in the carbonization process is heat-treated is above 2400°C, there is an advantage that the thermal diffusivity of the obtained graphite sheet is good, and when it is below 3300°C, there is an advantage that the sublimation of the graphite component in the graphitization furnace can be suppressed. The graphitization step is performed under reduced pressure or in an inert gas, and argon gas or helium gas can be used appropriately as the inert gas.

[0114] In the graphitization step, a rectangular carbon film may be graphitized while being stacked on a graphite sheet, a rolled carbon film may be graphitized while being rolled, or a film may be unrolled from a rolled carbon film and graphitized continuously.

[0115] In the graphitization process, the heating rate when the carbonaceous film is heated to the maximum temperature is not particularly limited, but from the viewpoint of providing a graphite sheet with good productivity, it is preferably 0.2°C / min or more, more preferably 0.3°C / min or more, further preferably 0.4°C / min or more, and further more preferably 0.5°C / min or more. When heat treatment (graphitization) is performed at a heating rate of 0.2°C / min or more, a carbonaceous film in which excessive foaming does not occur in the obtained graphite sheet can be said to be a carbonaceous film with excellent productivity, and a polyimide film that can provide such a carbonaceous film can be said to be a polyimide film with excellent productivity.

[0116] The carbonaceous film obtained by carbonizing the polyimide film has a certain degree of disordered orientation, similar to the polyimide film. Even when the carbonaceous film with a certain degree of disordered orientation is heat-treated (graphitized) at a high heating rate of 0.2°C / min or more in the graphitization process, the exhaust gas is easily discharged, and the foaming of the obtained graphite sheet can be suppressed, so that the graphite sheet can be provided with good productivity.

[0117] (Calendering process)

[0118] The calendering process is a process for calendering the graphite sheet obtained by the graphitization process (graphite sheet before calendering). The calendering process can also be said to be a process for obtaining a graphite sheet after calendering, or it can be said to be a compression process. The graphite sheet before calendering is in a foamed state due to the influence of the exhaust gas generated by the graphitization process, etc., and sometimes has an excessive thickness that is not suitable for implementation, but by performing the calendering process, the thickness of the graphite sheet can be adjusted, and in addition, flexibility can be imparted. In the calendering process, the method for calendering the graphite sheet is not particularly limited, and for example, a method of calendering using a metal roller or the like can be cited. The calendering process can be performed in a state where the manufactured graphite sheet is cooled to room temperature, or it can be performed continuously with the graphitization process.

[0119] One embodiment of the present invention may include the following configurations.

[0120] [1] A polyimide film for a graphite sheet, comprising an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA) and 0 to 50 mol % of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mol % of the total amount of the acid dianhydride component, and the diamine component contains 50 to 100 mol % of 4,4'-diaminodiphenyl ether (ODA) and 0 to 50 mol % of 2,2 - 0 to 50 mol% of bis[4-(4-aminophenoxy)phenyl]propane (BAPP); the total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component; and the polyimide film for the graphite sheet contains 0.1 to 5.0 wt% of the organic phosphorus compound in 100 wt% of the total amount of the polyimide film.

[0121] [2] The polyimide film for a graphite sheet according to [1], comprising 100 mol % of pyromellitic dianhydride (PMDA) as the acid dianhydride component, and 50 to 99 mol % of 4,4'-diaminodiphenyl ether (ODA) and 1 to 50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) as the diamine component.

[0122] [3] The polyimide film for a graphite sheet according to [1], comprising 100 mol% of 4,4'-diaminodiphenyl ether (ODA) as the diamine component, and comprising 50 to 99 mol% of pyromellitic dianhydride (PMDA), 1 to 50 mol% of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) as the acid dianhydride component. [4] The polyimide film for a graphite sheet according to any one of [1] to [3], having a thickness of 80 to 200 μm.

[0123] [5] The polyimide film for a graphite sheet according to any one of [1] to [4], wherein the organic phosphorus compound comprises an organic phosphorus compound having a valence of phosphorus of five.

[0124] [6] The polyimide film for a graphite sheet according to any one of [1] to [5], wherein the temperature at which the weight loss rate of the organic phosphorus compound reaches 5% in TG-DTA measurement is 200° C. or higher.

[0125] [7] A graphite sheet comprising the polyimide film for a graphite sheet according to any one of [1] to [6] as a raw material.

[0126] [8] A method for producing a polyimide film, comprising: mixing an acid dianhydride component and a diamine component to obtain a polyamic acid; and

[0127] A step of adding 0.1 to 5.0 wt % of an organic phosphorus compound to 100 wt % of the polyamic acid, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in the total amount of 100 mol % of the acid dianhydride component, and the diamine component contains 4,4'-diamine in the total amount of 100 mol % of the diamine component. 50 to 100 mol% of aminodiphenyl ether (ODA), 0 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), and the total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to the total amount of 200 mol% of the acid dianhydride component and the diamine component.

[0128] [9] A method for producing a graphite sheet, comprising the step of heat-treating a polyimide film for a graphite sheet at a temperature of 2400° C. or higher, wherein the polyimide film for a graphite sheet is a polyimide film made of an acid dianhydride component and a diamine component as raw materials, wherein the acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA) and 0 to 50 mol % of at least one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) in 100 mol % of the total amount of the acid dianhydride components, and the diamine component contains 4,4'-diaminodiphenylamine in 100 mol % of the total amount of the diamine components. The present invention relates to a graphite sheet having a polyimide film, wherein the content of the organic phosphorus compound is 0.1-5.0 wt % and the organic phosphorus compound is 0.1-10 mol % of an organic ether (ODA), and 0-50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP). The total amount of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 200 mol % of the total amount of the acid dianhydride component and the diamine component.

[0129]

[10] A method for producing a graphite sheet according to [9], wherein the polyimide film for the graphite sheet contains 100 mol % of pyromellitic dianhydride (PMDA) as the acid dianhydride component, and contains 50 to 99 mol % of 4,4'-diaminodiphenyl ether (ODA) and 1 to 50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) as the diamine component.

[0130]

[11] A method for producing a graphite sheet according to [9], wherein the polyimide film for the graphite sheet contains 100 mol % of 4,4'-diaminodiphenyl ether (ODA) as the diamine component, and contains 50 to 99 mol % of pyromellitic dianhydride (PMDA), 1 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) as the acid dianhydride component.

[0131]

[12] The method for producing a graphite sheet according to any one of [9] to

[11] , wherein the polyimide film for the graphite sheet has a thickness of 80 to 200 μm.

[0132]

[13] The method for producing a graphite sheet according to any one of [9] to

[12] , wherein the polyimide film for the graphite sheet contains an organic phosphorus compound having a phosphorus valence of five as the organic phosphorus compound.

[0133]

[14] The method for producing a graphite sheet according to any one of [9] to

[13] , wherein the temperature at which the weight loss rate of the organic phosphorus compound contained in the polyimide film for the graphite sheet reaches 5% in TG-DTA measurement is 200° C. or higher.

[0134] The present invention is not limited to the above-described embodiments, and various modifications can be made within the scope of the claims. Embodiments obtained by appropriately combining technical means disclosed in different embodiments are also included in the technical scope of the present invention.

[0135] Hereinafter, the present invention will be described in more detail with reference to Examples, but the present invention is not limited to the following Examples.

[0136] Example

[0137] Hereinafter, each evaluation method in Examples and Comparative Examples will be described.

[0138] <Thickness of graphite sheet before rolling>

[0139] The thickness of the graphite sheet before calendering is measured by the following method. For the graphite sheet before calendering, the thickness of the four corners and one central part of the graphite sheet is measured using a micrometer manufactured by Mitutoyo. Here, "one central part" means the position of the intersection of the diagonal lines drawn from the four measuring parts at each corner to the measuring parts at the diagonal angles in the obtained graphite sheet. Then, the average value of the measured values ​​of the thickness of the total of five parts (four corners and one central part) is taken as the thickness of the graphite sheet before calendering. It should be noted that the four corners refer to the vertices of the rectangular graphite sheet before calendering.

[0140] <Thickness of Graphite Sheet after Rolling>

[0141] The thickness of the rolled graphite sheet is measured by the following method. For the rolled graphite sheet, a micrometer manufactured by Mitutoyo is used to measure the thickness of the four corners and one center of the graphite sheet. Here, "one center" means the position of the intersection of the diagonal lines drawn from the four measurement points at each corner to the measurement points at the diagonal angles in the obtained graphite sheet. Then, the average value of the measured values ​​of the thickness of the total of five locations (four corners and one center) is taken as the thickness of the rolled graphite sheet. It should be noted that the four corners refer to the vertices of the rolled graphite sheet as a rectangular shape.

[0142] <Thermal diffusivity of rolled graphite sheet>

[0143] The thermal diffusivity of the rolled graphite sheet was measured by the following method. The thermal diffusivity was determined by cutting a sample of the rolled graphite sheet into a square shape of 30 mm × 30 mm, and measuring the thermal diffusivity under the condition of 25°C atmosphere and 75 Hz frequency using the "Thermowave Analyzer TA3" of Bethel Co., Ltd. It should be noted that the sample was made by punching the central part of the rolled graphite sheet as the measurement object with a Thomson knife. Here, the "central part" refers to the part that is in the center of the rolled graphite sheet in the width direction and also in the center in the length direction.

[0144] <Density of Graphite Sheet after Rolling>

[0145] The density of the rolled graphite sheet is measured by the following method. The central portion of the rolled graphite sheet is punched into a 30 mm × 30 mm square to obtain a sample. Thereafter, the weight of the sample is measured. Based on the measured value of the weight and the thickness of the sample measured by the method described in the above <Thickness of the rolled graphite sheet>, the density of the rolled graphite sheet is calculated by the following formula:

[0146] Density of the rolled graphite sheet (g / cm 3 ) = weight of the graphite sheet after rolling (g) / (area of ​​the graphite sheet after rolling (cm 2 )×thickness of the graphite sheet after rolling (cm).

[0147] (Example 1)

[0148] <Manufacturing of polyimide film>

[0149] 90 mol% of pyromellitic dianhydride (PMDA) and 10 mol% of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) were dissolved in a dimethylformamide solution in which 100 mol% of 4,4'-diaminodiphenyl ether (ODA) was dissolved to obtain a polyamic acid solution containing 18.5 wt% of polyamic acid. Triphenyl phosphate (TPP, valence of phosphorus 5, temperature at which weight loss rate becomes 5% in TG-DTA measurement is 220°C) as an organic phosphorus compound was added to the obtained polyamic acid solution in a manner that the concentration of the triphenyl phosphate was 0.3 wt% relative to 100 wt% of the solid content (polyamic acid) of the polyamic acid solution, and further, calcium hydrogen phosphate (inorganic particles) with an average particle size of 2.2 μm was added in a manner that the concentration of the calcium hydrogen phosphate was 0.08 wt% relative to 100 wt% of the solid content (polyamic acid) of the polyamic acid solution. The polyamic acid solution was cooled, and an imidization catalyst containing 1 equivalent of acetic anhydride, 1 equivalent of isoquinoline, and 1 equivalent of dimethylformamide relative to the carboxylic acid group contained in the polyamic acid was added and degassed to obtain a polyamic acid solution (mixed solution) containing an imidization catalyst.

[0150] Next, the mixed solution is applied to an aluminum foil in such a manner that the thickness after drying becomes 135 μm to obtain a mixed solution layer. The mixed solution layer on the aluminum foil is dried using a hot air oven and a far infrared heater. The drying conditions are as follows. First, the mixed solution layer on the aluminum foil is dried in a hot air oven at 120°C for 440 seconds to form a self-supporting gel film. The gel film is peeled off from the aluminum foil and fixed in a frame. Furthermore, the gel film is dried by stepwise heating in a hot air oven at 120°C for 60 seconds, 275°C for 72 seconds, 400°C for 77 seconds, 450°C for 93 seconds, and in a far infrared heater at 460°C for 40 seconds to prepare a polyimide film (A) with a thickness of 135 μm.

[0151] <Manufacturing of graphite sheet>

[0152] A polyimide film (A) cut into a size of 200 mm × 200 mm is sandwiched with a graphite sheet of a size of 220 mm × 220 mm (one polyimide film and one graphite sheet are alternately stacked) to obtain a laminate. The laminate is set in a carbonization device (carbonization device manufactured by Kurata Giken Co., Ltd.) (in a heating space). Under a vacuum atmosphere, the heating space in the carbonization device in which the above-mentioned laminate is set is heated to 600°C at a heating rate of 0.4°C / min, and then maintained at 600°C for 1 hour. Thereafter, the heating space in the carbonization device is heated to 1000°C at a heating rate of 0.4°C / min, and the above-mentioned laminate (polyimide film in the laminate) is heat-treated (carbonized) at 1000°C for 30 minutes to obtain a carbonaceous film.

[0153] The obtained carbonaceous film was cooled to room temperature (23°C) and rolled into a roll with an inner diameter of 100 mm to obtain a roll of carbonaceous film. The roll of the aforementioned carbonaceous film was placed on the furnace bed of a graphitization furnace (graphitization furnace manufactured by Kurata Giken Co., Ltd.) in a manner perpendicular to the width direction. In the temperature range below 2200°C, it was under reduced pressure. In the temperature range above 2200°C, it was under an argon atmosphere. After heating to 2900°C (the maximum graphitization temperature) at a heating rate of 0.3°C / min, it was maintained at 2900°C for 30 minutes to produce a graphitized film (graphite sheet before calendering). The measurement results of the thickness of the obtained graphite sheet before calendering are shown in Table 1.

[0154] The obtained graphitized film was cooled to room temperature and rolled using a 2-ton precision roller press (gap type) manufactured by THANK-METAL CO., LTD. to obtain a graphite sheet (rolled graphite sheet). The thickness, thermal diffusivity and density of the obtained rolled graphite sheet were measured and evaluated. The results are shown in Table 1.

[0155] (Examples 2-3, Comparative Example 1)

[0156] A polyimide film was prepared in the same manner as in Example 1, except that the amount of organic phosphorus compound added and / or the average particle size of inorganic particles were changed as shown in Table 1, and the polyimide film was heat-treated to obtain a graphite sheet. The various physical properties of the obtained graphite sheet were measured and evaluated. The results are shown in Table 1.

[0157] (Example 4)

[0158] In the manufacture of polyimide film, 100 mol% of pyromellitic dianhydride (PMDA) is dissolved in a dimethylformamide solution dissolved with 85 mol% of 4,4'-diaminodiphenyl ether (ODA) and 15 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), to obtain a polyamic acid solution containing 18.5 wt% of polyamic acid. Triphenyl phosphate (TPP) as an organic phosphorus compound is added to the obtained polyamic acid solution in a manner that the concentration of the triphenyl phosphate is 0.3 wt% relative to 100 wt% of the solid content (polyamic acid) of the polyamic acid solution, and further, calcium hydrogen phosphate (inorganic particles) with an average particle size of 2.2 μm is added in a manner that the concentration of the calcium hydrogen phosphate is 0.08 wt% relative to 100 wt% of the solid content (polyamic acid) of the polyamic acid solution.

[0159] (Examples 5 to 6, Comparative Example 2)

[0160] A polyimide film was prepared in the same manner as in Example 4 except that the amount of organic phosphorus compound added and / or the average particle size of inorganic particles were changed to those shown in Table 2, and then heat-treated to obtain a graphite sheet. The various physical properties of the obtained graphite sheet were measured and evaluated. The results are shown in Table 1.

[0161] (Comparative Example 3)

[0162] A polyimide film was prepared in the same manner as in Example 2 except that 90 mol% of pyromellitic dianhydride (PMDA) was used, 100 mol% of PMDA was used, and 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) was not used. The polyimide film was heat-treated to obtain a graphite sheet. The various physical properties of the obtained graphite sheet were measured and evaluated. The results are shown in Table 1.

[0163] [Table 1]

[0164]

[0165] 〔Summarize〕

[0166] The following can be clearly seen from Table 1.

[0167] According to Examples 1 to 3, it can be seen that the graphite sheet obtained by heat-treating a polyimide film containing 90 mol% (within the range of 50 to 100 mol%) of PMDA as an acid dianhydride component, 10 mol% (within the range of 0 to 50 mol%) of BTDA, and 100 mol% (within the range of 50 to 100 mol%) of ODA as a diamine component, and containing 0.3 to 1.1 wt% (within the range of 0.1 to 5.0 wt%) of an organic phosphorus compound, has a thickness of 135 μm before heat treatment. Although the thickness is large, the thickness of the obtained graphite sheet before rolling is very thin, and the graphite sheet is excellent in productivity. In addition, it can be seen from the comparison between Examples 1 to 3 and Comparative Example 1 that a graphite sheet having a higher density can be provided by making the polyimide film contain an organic phosphorus compound.

[0168] According to Examples 4 to 6, in terms of the polyimide film, the graphite sheet obtained by heat-treating the polyimide film containing 100 mol% (within the range of 50 to 100 mol%) of PMDA as an acid dianhydride component, 85 mol% (within the range of 50 to 100 mol%) of ODA as a diamine component, and 15 mol% (within the range of 0 to 50 mol%) of BAPP, and containing 0.3 to 1.1 wt% (within the range of 0.1 to 5.0 wt%) of an organic phosphorus compound, has a thickness of 135 μm before the heat treatment. Although the thickness is large, the thickness of the graphite sheet obtained by heat-treating at a high temperature increase rate of 0.5°C / min before rolling is very thin. That is, it is known that the graphite sheet is excellent in productivity, such as no excessive foaming, even when heat-treated at a high temperature increase rate. In addition, according to the comparison between Examples 4 to 6 and Comparative Example 2, it can be seen that by making the polyimide film contain an organic phosphorus compound, a graphite sheet with a higher density can be provided.

[0169] In addition, according to Comparative Example 3, for a polyimide film that does not use a monomer having an effect of disturbing the orientation of the polyimide film, such as BTDA, ODPA, or BAPP, as a raw material, when the temperature is increased at a high temperature increase rate of 0.5°C / min, the surface of the obtained graphite sheet is greatly foamed, and the thickness before rolling is too large, so it is substantially impossible to perform heat treatment at such a high temperature increase rate. It is also known that the density of the obtained graphite sheet is also low, and a graphite sheet with a high density cannot be provided.

[0170] The above results show that the polyimide film according to one embodiment of the present invention can provide a high-density graphite sheet, particularly a high-density thick graphite sheet, with good productivity.

[0171] Industrial Applicability

[0172] The polyimide film according to one embodiment of the present invention can provide a high-density graphite sheet with good productivity. Such a high-density graphite sheet can be suitably used as a heat dissipation member of electronic devices, especially thin electronic devices.

Claims

1. A polyimide film for a graphite sheet, which is a polyimide film made of an acid dianhydride component and a diamine component, The acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA), based on 100 mol % of the total amount of the acid dianhydride component. The diamine component contains 50 to 100 mol % of 4,4′-diaminodiphenyl ether (ODA), 0 to 50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), based on 100 mol % of the total amount of the diamine component. The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to the total amount of the acid dianhydride component and the diamine component (200 mol%). The polyimide film contains 0.1 to 5.0 wt % of the organic phosphorus compound based on 100 wt % of the total amount of the polyimide film.

2. The polyimide film for a graphite sheet according to claim 1, wherein The dianhydride component contains 100 mol% of pyromellitic dianhydride (PMDA), and the diamine component contains 50 to 99 mol% of 4,4'-diaminodiphenyl ether (ODA) and 1 to 50 mol% of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP).

3. The polyimide film for a graphite sheet according to claim 1, wherein The invention comprises 100 mol% of 4,4'-diaminodiphenyl ether (ODA) as the diamine component, and 50 to 99 mol% of pyromellitic dianhydride (PMDA), and 1 to 50 mol% of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) as the acid dianhydride component.

4. The polyimide film for graphite sheet according to claim 1, which has a thickness of 80 to 200 μm.

5. The polyimide film for a graphite sheet according to claim 1, wherein The organic phosphorus compound includes one in which phosphorus has a valence of five.

6. The polyimide film for a graphite sheet according to claim 1, wherein The temperature at which the weight loss rate of the organic phosphorus compound reaches 5% in TG-DTA measurement is 200° C. or higher. 7 . A graphite sheet comprising the polyimide film for a graphite sheet according to claim 1 as a raw material.

8. A method for producing a polyimide film, comprising: A step of mixing an acid dianhydride component and a diamine component to obtain a polyamic acid; and a step of adding 0.1 to 5.0 wt % of an organic phosphorus compound to 100 wt % of the polyamic acid; The acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA), based on 100 mol % of the total amount of the acid dianhydride component. The diamine component contains 50 to 100 mol % of 4,4′-diaminodiphenyl ether (ODA), 0 to 50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), based on 100 mol % of the total amount of the diamine component. The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to 200 mol% of the total amount of the acid dianhydride component and the diamine component.

9. A method for producing a graphite sheet, comprising the step of heat treating a polyimide film for the graphite sheet at a temperature above 2400° C. The polyimide film used for the graphite sheet is a polyimide film made of dianhydride components and diamine components. The acid dianhydride component contains 50 to 100 mol % of pyromellitic dianhydride (PMDA), 0 to 50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA), based on 100 mol % of the total amount of the acid dianhydride component. The diamine component contains 50 to 100 mol % of 4,4′-diaminodiphenyl ether (ODA), 0 to 50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP), based on 100 mol % of the total amount of the diamine component. The total content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), the 4,4'-oxydiphthalic dianhydride (ODPA) and the 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) is 1 to 50 mol% relative to the total amount of the acid dianhydride component and the diamine component (200 mol%). The polyimide film contains 0.1 to 5.0 wt % of the organic phosphorus compound based on 100 wt % of the total amount of the polyimide film.

10. The method for producing a graphite sheet according to claim 9, wherein: The polyimide film for graphite sheet contains 100 mol % of pyromellitic dianhydride (PMDA) as the dianhydride component, 50-99 mol % of 4,4'-diaminodiphenyl ether (ODA) and 1-50 mol % of 2,2-bis[4-(4-aminophenoxy)phenyl]propane (BAPP) as the diamine component.

11. The method for producing a graphite sheet according to claim 9, wherein: The polyimide film for the graphite sheet contains 100 mol % of 4,4'-diaminodiphenyl ether (ODA) as the diamine component, and contains 50-99 mol % of pyromellitic dianhydride (PMDA), 1-50 mol % of at least any one of 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA) and 4,4'-oxydiphthalic dianhydride (ODPA) as the acid dianhydride component.

12. The method for producing a graphite sheet according to claim 9, wherein: The thickness of the polyimide film used for the graphite sheet is 80-200 μm.

13. The method for producing a graphite sheet according to claim 9, wherein: The polyimide film for a graphite sheet contains the organic phosphorus compound having a valence of phosphorus of five as an organic phosphorus compound.

14. The method for producing a graphite sheet according to claim 9, wherein: The temperature at which the weight loss rate of the organic phosphorus compound contained in the polyimide film for the graphite sheet reaches 5% in TG-DTA measurement is 200° C. or higher.

Citation Information

Patent Citations

  • Polyimide film and method for producing the same

    JP2020164611A

Cited By

  • Polyimide film for graphite sheets and graphite sheets manufactured from the same

    JP2026507032A