New application of skin transplantation hydrogel
The skin grafting hydrogel prepared by modified gelatin and modified silk protein solves the problem of difficult skin grafting during external auditory canal reconstruction, achieves good skin grafting growth and reduces the surgical failure rate, and provides a method for treating minor irregularities. Effective repair material for surface surfaces.
Patent Information
- Application Number
- CN202410830497.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
AI Technical Summary
During the external auditory canal reconstruction surgery, the surgical cavity is narrow, the transplant wound is annular, and the transplant bed is a bone surface, which makes skin grafting difficult and often causes shedding or necrosis, resulting in a high surgical failure rate.
A skin grafting hydrogel prepared by modified gelatin and modified silk protein. Through the preparation of modified gelatin, the preparation of modified silk protein and the preparation method of skin grafting hydrogel, the skin grafting hydrogel is formed with adhesiveness, antioxidant and support. A cell scaffold for cell migration, used for the repair of small irregular or annular skin defects.
It effectively avoids the stenosis of the external auditory canal after skin transplantation, and the skin graft grows well, which significantly reduces the surgical failure rate and provides an effective repair material for more difficult external auditory canal reconstruction.
Smart Images

Figure CN118750646A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biochemistry, and in particular relates to a new use of a skin transplantation hydrogel. Background Art
[0002] External auditory canal plasty is to reconstruct the external auditory canal and restore its sound transmission function to the middle ear to improve the patient's hearing. External auditory canal plasty can be performed simultaneously with primary auricular plasty, or it can be performed separately or completed together with secondary auricular plasty. When reconstructing the external auditory canal, skin grafting is generally performed on the widened bony surface of the external auditory canal. Since the grafted surface is a small irregular surface or a small irregular annular surface, it is a difficult transplantation situation.
[0003] At present, after external auditory canal reconstruction surgery, skin grafts are required for the enlarged bony external auditory canal annular wound to ensure good epithelialization of the external auditory canal and prevent the external auditory canal from closing again, which would lead to surgical failure. There are three obvious limitations in the current skin grafting of external auditory canal reconstruction surgery. The first is the narrow surgical cavity, the second is the circular shape of the transplanted wound, and the third is the bone surface of the transplant bed. At the same time, establishing a good blood supply to the transplanted skin on the transplant bed is critical to the survival of the transplanted skin and the healthy epithelialization of the surgical cavity.
[0004] Because the surgical cavity is small, if a full-thickness skin graft is used, the space left in the external auditory canal is too small (or there is not enough space to complete a full-thickness skin graft), so partial-thickness skin grafts are currently more widely used. Also because the surgical cavity is small, the decellularized collagen matrix that provides support (blood supply and cell migration) for partial-thickness skin grafts in clinical practice is difficult to use, such as Plastic Surgery Matrix, at least 0.7 cm thick.
[0005] The skin transplant interface is annular, which causes the transplanted skin to not fit the transplant bed as firmly as the flat wound surface, especially the upper side of the annular skin graft. Because the acellular collagen matrix currently used in clinical practice is relatively thick and has no obvious adhesion properties, it is impossible to make the skin graft fit the external auditory canal firmly by acting on the interface between the transplanted skin and the bony external auditory canal during external auditory canal reconstruction. The current clinical method for making the transplanted skin fit the bone surface is to use gelatin sponge or expanded sponge (Merocel) to fill the external auditory canal cavity, providing support from the outside to press the skin graft firmly onto the bone surface. The above sponge is used for 1-2 weeks after surgery, and the replacement frequency is adjusted according to the healing condition.
[0006] Compared with the soft tissue bed, it is more difficult for the bone surface to attach the transplanted skin, and the bone surface transplant bed itself lacks the ability to provide blood supply for the transplanted skin.
[0007] In summary, due to the above limitations, the skin grafts in the external auditory canal reconstruction surgery often fall off or necrotize, and then the granulation tissue in the external auditory canal proliferates and scars grow, leading to the narrowing or atresia of the external auditory canal again, and finally the failure of the operation. The failure rate of external auditory canal reconstruction surgery is as high as 33-50%.
[0008] The skin graft hydrogel is an adhesive between the skin graft and the defective skin. The present invention intends to provide a skin graft hydrogel that can be used for skin defect repair, especially for external auditory canal skin grafting in more difficult bone surface skin lesions and more difficult external auditory canal reconstruction. Summary of the invention
[0009] The technical problem solved by the present invention is to provide a new use of skin transplant hydrogel. Specifically, it is the use of the skin transplant hydrogel in the preparation of materials for repairing skin defects of small irregular surfaces or small irregular annular surfaces; further, it is for external auditory canal skin grafting in external auditory canal reconstruction surgery, which is more difficult to repair.
[0010] The skin transplantation hydrogel involved in the present invention is prepared by the following preparation method, which comprises the following steps:
[0011] A. Preparation of modified gelatin (GelMA):
[0012] A1) dissolving gelatin in a phosphate buffered saline (PBS) at 40° C.-65° C., and then slowly adding methacrylic anhydride to the solution obtained in step A1) to react;
[0013] A2) After the reaction, adding phosphate buffered saline (PBS) dilution solution to step A1) to stop the reaction;
[0014] A3) the reaction solution in step A2) is transferred to a dialysis device for dialysis, and the dialysate is freeze-dried to obtain modified gelatin;
[0015] B. Preparation of modified silk protein (SFMA):
[0016] B1) removing sericin from silk cocoons with a Na2CO3 aqueous solution, then repeatedly washing with deionized water to remove sericin on the surface of silk, and drying to obtain silk fibroin;
[0017] B2) dissolving the silk fibroin obtained in step B1) with a lithium bromide (LiBr) aqueous solution, then adding glycidyl methacrylate (GMA) and reacting under nitrogen protection;
[0018] B3) diluting the solution obtained in step B2) with deionized water, filtering to remove impurities, and dialyzing to remove excess lithium bromide (LiBr) and glycidyl methacrylate (GMA);
[0019] B4) freeze-drying the dialysate to obtain modified silk protein;
[0020] C. Preparation of hydrogel for skin transplantation
[0021] C1) preparing a reaction solution: dissolving tannic acid and zinc chloride in deionized water, then adding modified gelatin and modified silk protein to fully dissolve them, and finally adding phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (Lap) to obtain a mixed solution;
[0022] C2) The mixed solution obtained in step C1) is irradiated under a blue light ultraviolet lamp of 365-405 nm to form a hydrogel.
[0023] In the preparation of modified gelatin (GelMA) in step A of the above technical solution:
[0024] The dissolving temperature in step A1) is 40°C;
[0025] The ratio of gelatin, phosphate buffered saline solution and methacrylic anhydride in step A1) is:
[0026] For every 1 g of gelatin, add 50-100 mL of phosphate buffered saline and 0.2-0.8 mL of methacrylic anhydride.
[0027] Preferably, 100 mL of phosphate buffered saline and 0.6 mL of methacrylic anhydride are added to every 1 g of gelatin.
[0028] The reaction in step A1) is carried out by stirring the mixture at water bath temperature.
[0029] The reaction in step A1) is carried out in a water bath at 40-65° C. for 2-4 hours.
[0030] Preferably, the reaction in step A1) is carried out in a water bath at 40° C. for 3 hours.
[0031] In step A2), the amount of PBS diluted solution added is calculated based on the amount of gelatin fed: 100-200 mL of PBS diluted solution is added for every 1 g of gelatin.
[0032] Preferably, the amount of PBS dilution solution added in step A2) is calculated based on the amount of gelatin fed: 100 mL of PBS dilution solution is added for every 1 g of gelatin.
[0033] The pH of the phosphate buffered saline solution in step A1) and step A2) is 7.4.
[0034] The dialysis device or dialysis bag in step A3) is a dialysis bag.
[0035] Step A3) The dialysis conditions are: molecular weight cut-off 5-14 kDa, and dialysis is performed in deionized water at 40-50° C. for 2-3 days.
[0036] Preferably, the dialysis condition in step A3) is a molecular weight cut-off of 14 kDa, and dialysis is performed in deionized water at 40° C. for 3 days.
[0037] In the preparation of modified silk protein (SFMA) in step B of the above technical solution:
[0038] Step B1) The concentration of the Na2CO3 aqueous solution is 0.4-1% (w / v).
[0039] Preferably, the concentration of the Na2CO3 aqueous solution in step B1) is 0.5% (w / v).
[0040] Natural silkworm silk is composed of fibroin, which is wrapped by sericin. The purpose of using Na2CO3 aqueous solution to treat is to remove sericin. Specifically, in step B1), the silkworm cocoon is boiled for 0.5-1 hour under boiling conditions to remove sericin using Na2CO3 aqueous solution.
[0041] Preferably, in step B1), the silk cocoons are boiled for 1 hour using a Na2CO3 aqueous solution to remove sericin.
[0042] Step B2) The ratio of the silk protein, lithium bromide (LiBr) aqueous solution, and glycidyl methacrylate (GMA) is as follows: 50-100 mL 9.3 M lithium bromide (LiBr) aqueous solution and 2-8 mL glycidyl methacrylate (GMA) are added to every 10 g of silk protein.
[0043] Preferably, in step B2), the ratio of the silk protein, lithium bromide (LiBr) aqueous solution, and glycidyl methacrylate (GMA) is as follows: 75 mL of 9.4 M lithium bromide (LiBr) aqueous solution and 2 mL of glycidyl methacrylate (GMA) are added to every 10 g of silk protein.
[0044] The nitrogen protection conditions in step B2) are 100-200 rpm and 60-70° C. Preferably, the nitrogen protection conditions in step B2) are 400 rpm and 60° C.
[0045] The reaction time of step B2) is 2-4 hours. Preferably, the reaction time of step B2) is 3 hours.
[0046] Step B3) The filtration to remove impurities is performed by using a sterile syringe with a 0.22-0.45 μm external filter.
[0047] Step B3) The filtration to remove impurities is performed by using a sterile syringe with a 0.22 μm or 0.45 μm external filter.
[0048] The dialysis condition in step B3) is a molecular weight cut-off of 5-14 kDa. Preferably, the dialysis condition in step B3) is a molecular weight cut-off of 14 kDa.
[0049] Step B3) During the dialysis, the dialysis environment temperature is controlled to be lower than 30°C.
[0050] Step B3) dilutes the solution obtained in step B2) with deionized water to 5-6 times the volume.
[0051] In step B, the stirring speed of the dissolved protein must be strictly controlled, the mixed solution must be diluted before dialysis, and the dialysis environment temperature must be controlled. The above parameter control is to avoid crystallization of silk fibroin caused by rapid stirring, high concentration dialysis and high temperature.
[0052] In the preparation of the skin transplantation hydrogel in step C of the above technical scheme:
[0053] Step C1) prepares the reaction solution according to the following ratio: add 5-10 mg of tannic acid (TA) and 2-4 mg of zinc chloride to each 2 ml of deionized water to dissolve, then add 100-200 mg of modified gelatin, 200-300 mg of modified silk protein to fully dissolve, and finally add 20-50 μL of 0.5-1 wt% Lap. Preferably, step C1) prepares the reaction solution according to the following ratio: add 6 mg of tannic acid (TA) and 2 mg of zinc chloride to each 2 ml of deionized water to dissolve, then 200 mg of modified gelatin and 200 mg of modified silk protein to fully dissolve, and finally add 50 μL of 0.05 wt% Lap.
[0054] Step C2) The irradiation conditions under the blue light ultraviolet lamp are: wavelength 365 or 450nm, irradiation 1-3min.
[0055] Preferably, in step C2), the irradiation conditions under the blue light ultraviolet lamp are: wavelength 405nm, irradiation 1min.
[0056] The skin transplantation hydrogel of the present invention is prepared by using modified gelatin and modified silk protein as main raw materials. The safety of the hydrogel of the present invention is proved by hemolysis experiment and toxicity experiment. The hydrogel of the present invention is applied to the repair of tiny irregular surfaces with high difficulty in skin lesion transplantation, such as external auditory canal skin grafting in external auditory canal reconstruction. Because the skin transplantation hydrogel of the present invention has the functions of adhesion, anti-oxidation and cell scaffold supporting cell migration, the stenosis of the external auditory canal after skin transplantation is avoided, and the skin grafting grows well, so it has a good repair effect. The pre-protected hydrogel of the present invention is used in the preparation of materials for skin transplantation on tiny irregular surfaces, especially the protection hydrogel is used in the preparation of materials for external auditory canal skin grafting in external auditory canal reconstruction. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] Figure 1 .Hemolytic properties of different hydrogels.
[0058] in: Figure 1 a represents the hemolysis rate of hydrogels with different components relative to the positive control group in the hemolysis test; Figure 1 b shows the photograph of the experimental site of different gel centrifuge tubes during the hemolysis test.
[0059] Figure 2 . Live-dead staining fluorescence images and cell viability ratios of L929 cells treated with different hydrogels.
[0060] in: Figure 2 a) Live / dead staining results under fluorescence microscope for 24h / 48h; Figure 2 b) indicates the results of 24h CCK-8 cytotoxicity test; Figure 2 c) shows the results of CCK-8 cytotoxicity test at 48 h.
[0061] Figure 3 GSZT hydrogel was used for skin transplantation reconstruction of the external auditory canal of rats.
[0062] Figure 4 .GSZT hydrogel stress test results.
[0063] Figure 5 .Tensile test results of GSZT hydrogel. DETAILED DESCRIPTION
[0064] Below in conjunction with embodiment, the scheme of the present invention will be explained and described.It will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be regarded as limiting the scope of the present invention.In the embodiment, if no specific technology or condition is indicated, it is carried out according to the technology or condition described in the document in this area or according to the product specification.The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained by commercial purchase.
[0065] The following are the definitions of the English abbreviations and main terms used in this invention:
[0066] Modified gelatin is referred to as GelMA, methacrylic anhydride is referred to as MA, modified silk protein is referred to as SFMA, lithium bromide is referred to as LiBr, glycidyl methacrylate is referred to as GMA, skin transplantation hydrogel is referred to as GSZT, and phenyl (2,4,6-trimethylbenzoyl) lithium phosphate is referred to as Lap.
[0067] According to the inventor's previous screening of feed and preparation process parameters, a preparation method for the skin transplantation hydrogel of the present invention was obtained, and the steps are as follows:
[0068] A. Preparation of modified gelatin (GelMA):
[0069] A1) dissolving gelatin in a phosphate buffered saline solution (PBS, pH=7.4) at 40° C., and then slowly adding methacrylic anhydride (MA) to the solution obtained in step A1) to react;
[0070] A2) After the reaction, adding PBS dilution solution to step A1) to stop the reaction;
[0071] A3) the reaction solution in step A2) is transferred to a dialysis device for dialysis, and the dialysate is freeze-dried to obtain modified gelatin;
[0072] B. Preparation of modified silk protein (SFMA):
[0073] B1) removing sericin from silk cocoons with a Na2CO3 aqueous solution, then repeatedly washing with deionized water to remove sericin on the surface of silk, and drying to obtain silk fibroin;
[0074] B2) dissolving the silk fibroin obtained in step B1) with a lithium bromide (LiBr) aqueous solution, then adding glycidyl methacrylate (GMA) and reacting under nitrogen protection;
[0075] B3) diluting the solution obtained in step B2) with deionized water, filtering to remove impurities, and dialyzing to remove excess lithium bromide (LiBr) and glycidyl methacrylate (GMA);
[0076] B4) freeze-drying the dialysate to obtain modified silk protein;
[0077] C. Preparation of hydrogel for skin transplantation
[0078] C1) preparing a reaction solution: dissolving tannic acid and zinc chloride in deionized water, then adding modified gelatin and modified silk protein to fully dissolve them, and finally adding phenyl (2,4,6-trimethylbenzoyl) lithium phosphate (Lap) to obtain a mixed solution;
[0079] C2) The mixed solution obtained in step C1) is irradiated under a blue light ultraviolet lamp of 365-405 nm to form a hydrogel.
[0080] In the preparation of modified gelatin (GelMA) in step A of the above technical solution:
[0081] Step A1) the dissolving temperature is 40-65°C;
[0082] Preferably, the dissolving temperature in step A1) is 40°C;
[0083] The ratio of gelatin, phosphate buffered saline solution and methacrylic anhydride in step A1) is:
[0084] For every 1 g of gelatin, add 50-100 mL of phosphate buffered saline and 0.2-0.8 mL of methacrylic anhydride.
[0085] Preferably, 100 mL of phosphate buffered saline and 0.6 mL of methacrylic anhydride are added to every 1 g of gelatin.
[0086] The reaction in step A1) is carried out by stirring the mixture at water bath temperature.
[0087] The reaction in step A1) is carried out in a water bath at 40-65° C. for 2-4 hours.
[0088] Preferably, the reaction in step A1) is carried out in a water bath at 40° C. for 3 hours.
[0089] In step A2), the amount of PBS diluted solution added is calculated based on the amount of gelatin fed: 100-200 mL of PBS diluted solution is added for every 1 g of gelatin.
[0090] Preferably, the amount of PBS dilution solution added in step A2) is calculated based on the amount of gelatin fed: 100 mL of PBS dilution solution is added for every 1 g of gelatin.
[0091] The pH of the phosphate buffered saline solution in step A1) and step A2) is 7.4.
[0092] The dialysis device or dialysis bag in step A3) is a dialysis bag.
[0093] Step A3) The dialysis conditions are: molecular weight cut-off 5-14 kDa, and dialysis is performed in deionized water at 40-50° C. for 2-3 days.
[0094] Preferably, the dialysis condition in step A3) is a molecular weight cut-off of 14 kDa, and dialysis is performed in deionized water at 40° C. for 3 days.
[0095] In the preparation of modified silk protein (SFMA) in step B of the above technical solution:
[0096] Step B1) The concentration of the Na2CO3 aqueous solution is 0.4-1% (w / v).
[0097] Preferably, the concentration of the Na2CO3 aqueous solution in step B1) is 0.5% (w / v).
[0098] Natural silkworm silk is composed of fibroin, which is wrapped by sericin. The purpose of using Na2CO3 aqueous solution to treat is to remove sericin. Specifically, in step B1), the silkworm cocoon is boiled for 0.5-1 hour under boiling conditions to remove sericin using Na2CO3 aqueous solution.
[0099] Preferably, in step B1), the silk cocoons are boiled for 1 hour using a Na2CO3 aqueous solution to remove sericin.
[0100] Step B2) The ratio of the silk protein, lithium bromide (LiBr) aqueous solution, and glycidyl methacrylate (GMA) is as follows: 50-100 mL 9.3 M lithium bromide (LiBr) aqueous solution and 2-8 mL glycidyl methacrylate (GMA) are added to every 10 g of silk protein.
[0101] Preferably, in step B2), the ratio of the silk protein, lithium bromide (LiBr) aqueous solution, and glycidyl methacrylate (GMA) is as follows: 75 mL of 9.4 M lithium bromide (LiBr) aqueous solution and 2 mL of glycidyl methacrylate (GMA) are added to every 10 g of silk protein.
[0102] Step B2) The nitrogen protection conditions are 100-200rpm, 60-70°C.
[0103] Preferably, the nitrogen protection conditions in step B2) are 400 rpm and 60°C.
[0104] The reaction time of step B2) is 2-4h.
[0105] Preferably, the reaction time in step B2) is 3 h.
[0106] Step B3) The filtration to remove impurities is performed by using a sterile syringe with a 0.22-0.45 μm external filter.
[0107] Step B3) The filtration to remove impurities is performed by using a sterile syringe with a 0.22 μm or 0.45 μm external filter.
[0108] Step B3) The dialysis condition is a molecular weight cut-off of 5-14 kDa.
[0109] Preferably, the dialysis condition in step B3) is a molecular weight cut-off of 14 kDa.
[0110] Step B3) During the dialysis, the dialysis environment temperature is controlled to be lower than 30°C.
[0111] Step B3) dilutes the solution obtained in step B2) with deionized water to 5-6 times the volume.
[0112] In step B, the stirring speed of the dissolved protein must be strictly controlled, the mixed solution must be diluted before dialysis, and the dialysis environment temperature must be controlled. The above parameter control is to avoid crystallization of silk fibroin caused by rapid stirring, high concentration dialysis and high temperature.
[0113] In the preparation of the skin transplantation hydrogel in step C of the above technical scheme:
[0114] Step C1) Prepare the reaction solution according to the following ratio: add 5-10 mg of tannic acid (TA) and 2-4 mg of zinc chloride to every 2 ml of deionized water to dissolve, then add 100-200 mg of modified gelatin and 200-300 mg of modified silk protein to fully dissolve, and finally add 20-50 μL of 0.5-1 wt% Lap.
[0115] Preferably, in step C1), the reaction solution is prepared according to the following ratio: 6 mg of tannic acid (TA) and 2 mg of zinc chloride are added to every 2 ml of deionized water to dissolve, then 200 mg of modified gelatin and 200 mg of modified silk protein are fully dissolved, and finally 50 μL of 0.05 wt% Lap is added.
[0116] Step C2) The irradiation conditions under the blue light ultraviolet lamp are: wavelength 365 or 450nm, irradiation 1-3min.
[0117] Preferably, in step C2), the irradiation conditions under the blue light ultraviolet lamp are: wavelength 405nm, irradiation 1min.
[0118] The following experiment was used to demonstrate the beneficial effects of the hydrogel of the present invention. The skin transplantation hydrogel and the reference hydrogel in the experiment were prepared by the following method:
[0119] a. Preparation of GelMA:
[0120] First, 1 g of gelatin (Gel) was dissolved in 100 mL of phosphate buffered saline (PBS, pH = 7.4) at 60 ° C. Then 0.6 mL of methacrylic anhydride (MA) was slowly added to the gelatin solution, and the mixture was stirred in a 40 ° C water bath. After 3 hours of reaction, the solution was diluted with 100 mL of PBS to stop the reaction. Afterwards, the solution was transferred to a dialysis bag (molecular weight cutoff 14 kDa) and dialyzed in deionized water at 40 ° C for 3 days. Finally, the dialysate was freeze-dried to obtain GelMA and placed in a 4 ° C refrigerator for use.
[0121] b. Preparation of SFMA:
[0122] The silk cocoons were added to a 0.5% (w / v) Na2CO3 aqueous solution and boiled for 1 hour to remove the sericin, then washed repeatedly in deionized water until thoroughly cleaned and dried. Next, 10 g of silk protein was placed in a three-necked flask with 75 mL of 9.4 M lithium bromide (LiBr) aqueous solution, heated to 60 ° C and stirred continuously for 1 hour. After it was completely dissolved, 2 mL of glycidyl methacrylate (GMA) was added to the three-necked flask and reacted for 3 hours at 400 rpm and 60 ° C under nitrogen protection. After the reaction was completed, the mixed solution was diluted to 5-6 times the volume with deionized water, and impurities were removed using a sterile syringe with a 0.22 μm external filter head, and excess LiBr and GMA were dialyzed with a 14 kDa dialysis bag. Finally, the SFMA solution was freeze-dried to obtain pure SFMA powder.
[0123] Group A, Example 1 (GS hydrogel):
[0124] 200 mg GelMA and 200 mg SFMA were fully dissolved in 2 mL deionized water, and finally 50 μL 0.05 wt % Lap was added, and the mixed solution was irradiated under a 405 nm blue light UV lamp for 1 min to form a hydrogel.
[0125] Group B, Example 2 (GS / Zn hydrogel):
[0126] 2 mg zinc chloride, 200 mg GelMA, and 200 mg SFMA were fully dissolved in 2 mL deionized water, and finally 50 μL 0.05 wt % Lap was added, and the mixed solution was irradiated under a 405 nm blue light UV lamp for 1 min to form a hydrogel.
[0127] Group C, Example 3 (GS / TA hydrogel):
[0128] 6 mg tannic acid, 200 mg GelMA, and 200 mg SFMA were fully dissolved in 2 mL deionized water, and finally 50 μL 0.05 wt % Lap was added, and the mixed solution was irradiated under a 405 nm blue light UV lamp for 1 min to form a hydrogel.
[0129] Group D, Example 4 (GSZT hydrogel):
[0130] 6 mg tannic acid (TA) and 2 mg zinc chloride were dissolved in 2 ml deionized water, followed by the addition of 200 mg GelMA and 200 mg SFMA to fully dissolve, and finally 50 μL 0.05 wt % Lap was added, and the mixed solution was irradiated under a 405 nm blue light UV lamp for 1 min to form a hydrogel.
[0131] 1. Characterization of hydrogel:
[0132] Hemolysis test Figure 1 As shown, fresh red blood cells from SD rats were used in the experiment. The blood was centrifuged at 3000rpm for 10 minutes and then washed with saline, and the washing process was repeated 3 times. Saline mixed with 2% red blood cells was used for subsequent experiments. 0.5mL of GS hydrogel, GS / Zn hydrogel, GS / TA hydrogel and GSZT hydrogel were placed in centrifuge tubes containing 3mL of red blood cell saline. After incubation at 37℃ for 1 hour, the mixed solutions were centrifuged to remove the un-hemolyzed red blood cells. The absorbance of the supernatant at 545nm was measured by UV spectrophotometer. Saline and 0.1% Trition-X-100 solution were negative and positive controls, respectively. Figure 1 a represents the hemolysis rate of hydrogels with different components relative to the positive control group in the hemolysis test; Figure 1 b shows the photos of the experimental site of different gel centrifuge tubes during the hemolysis test. The final results show that none of the gels showed hemolysis, indicating excellent blood safety.
[0133] 2. Toxicity test:
[0134] CCK-8 cytotoxicity test: After disinfecting the gel with 75% alcohol, wash the gel with PBS. Add 0.1g / mL of each of the four gels to Rosell-Park-Memorial-Institute-1640 culture medium with 10% FBS and 1% penicillin-streptomycin and soak for 24 hours. L929 mouse fibroblasts (3000 cells / well) were cultured at 37°C in the above four different culture mediums for 24 hours / 48 hours. At the predetermined time, the CCK-8 reagent was added to the wells cultured with the four different gel extracts, incubated at 37°C for 1 hour, and finally the absorbance at 450nm was tested using an enzyme reader, and the cell viability was calculated with the control group (cells cultured in culture medium without hydrogel extract) as 100%.
[0135] Live / dead staining: After disinfecting the gel with 75% alcohol, wash the gel with PBS. Add 0.1g / mL of each of the four gels to Rosell-Park-Memorial-Institute-1640 culture medium with 10% FBS and 1% penicillin-streptomycin and soak for 24 hours. L929 mouse fibroblasts (3000 cells / well) were cultured at 37°C for 24 hours / 48 hours in the above four different culture mediums. The culture medium was removed at the predetermined time, and each well was washed with PBS to remove impurities 3 times. Live / dead dyes PI and AM were added to 10mL of PBS, and a mixture of live / dead dyes and PBS was added to each well. After staining for 20 minutes, the cells were photographed using a fluorescence microscope. Under a fluorescence microscope, living cells are stained green and dead cells are stained red.
[0136] like Figure 2 Cytotoxicity test CCK-8 and live-dead staining (FDA / PI) showed that Figure 2 a represents the live / dead staining results of 24h / 48h under a fluorescence microscope, showing that fibroblasts under the influence of different hydrogel components can survive well; Figure 2 b shows the results of the 24-hour CCK-8 cytotoxicity test, showing that the cell activity under the influence of the hydrogel was higher than 90% compared with the control group; Figure 2 c shows the results of the CCK-8 cytotoxicity test at 48 h. It can be seen that the cell activity under the influence of the hydrogel is higher than 90% compared with the control group. Figure 2 The results showed that L929 cells treated with different hydrogels grew well and the cell viability was greater than 80%, indicating that the hydrogels had good biocompatibility.
[0137] 3. External auditory canal test - usage:
[0138] GSZT hydrogel was applied to the contact surface between the skin graft and the transplanted surface, and the area was illuminated with 405nm blue ultraviolet light for 1 minute to check whether the skin graft and the transplanted surface tissue were firmly attached. Rats with only skin grafting without hydrogel were used as controls.
[0139] The results are as follows Figure 3 As shown in the figure, compared with the control group, GSZT hydrogel combined with skin graft had the best therapeutic effect on external auditory canal skin transplantation reconstruction in rats, avoiding the stenosis of the external auditory canal after skin transplantation and achieving good growth of the skin graft.
[0140] 4. GSZT hydrogel stress test results:
[0141] The pressure test was carried out in an Instron 5967 mechanical tester, with a gel diameter of 10 mm, a thickness of 20 mm, and a temperature of 25° C. The speeds were 5 mm / min, 50 mm / min, and 500 mm / min for 5 cycles, respectively, with a deformation of 50%.
[0142] The results are as follows Figure 4 As shown: diameter: 10mm, final compression plate height: 10mm, compression strain (displacement) at maximum load: -0.03218mm / mm, compression stress at maximum load: 0.00458MPa. The pressure test results show that the hydrogel has good impact resistance after gelation. The gel can maintain structural stability when subjected to impacts of different impulse sizes (speed 5-500mm / min) on the body surface, avoiding unexpected situations such as deformation or fragmentation after implantation on the body surface during use.
[0143] 5. GSZT hydrogel tensile test results:
[0144] The tensile test was carried out in an Instron 5967 mechanical tester, with a gel width of 3 mm, a thickness of 2 mm, a temperature of 25° C., a speed of 5 mm / min, and the test was carried out until the gel broke.
[0145] The results are as follows Figure 5 As shown: straight width: 3mm, thickness: 2mm, tensile stress at yield (zero slope): 0.1523MPa. Maximum load: 0.91378N. Maximum tensile strain (displacement): 246.78552%. The tensile test results show that the hydrogel has a certain deformation stability after gelation. The gel can maintain structural stability after being stretched to 3 times its length, avoiding unexpected situations such as breakage after implantation on the body surface.
[0146] In summary, the skin transplantation hydrogel of the present invention is prepared using modified gelatin and modified silk protein as main raw materials. The safety of the hydrogel of the present invention has been proved by hemolysis experiment and toxicity experiment. When the hydrogel of the present invention is applied to the external auditory canal skin transplantation reconstruction with high difficulty in skin lesion transplantation, the stenosis of the external auditory canal after skin transplantation is avoided, and the skin graft grows well, which provides a new option for clinical skin lesion repair, especially skin transplantation on tiny irregular surfaces, and even external auditory canal skin grafting in highly difficult external auditory canal reconstruction.
Claims
1. Application of skin transplantation hydrogel in the preparation of materials for repairing skin defects of small irregular surfaces or small irregular annular surfaces, characterized in that: The hydrogel is prepared by a method comprising the following steps: A. Preparation of modified gelatin: A1) dissolving gelatin in a phosphate buffered saline solution at 40° C. to 65° C., and then slowly adding methacrylic anhydride to the solution obtained in step A1) to react; A2) After the reaction, adding phosphate buffered saline dilution solution to step A1) to stop the reaction; A3) the reaction solution in step A2) is transferred to a dialysis device for dialysis, and the dialysate is freeze-dried to obtain modified gelatin; B. Preparation of modified silk protein: B1) removing sericin from silk cocoons with a Na2CO3 aqueous solution, then repeatedly washing with deionized water to remove sericin on the surface of silk, and drying to obtain silk fibroin; B2) dissolving the silk fibroin obtained in step B1) with a lithium bromide aqueous solution, then adding glycidyl methacrylate (GMA) and reacting under nitrogen protection; B3) diluting the solution obtained in step B2) with deionized water, filtering to remove impurities, and dialyzing to remove excess lithium bromide and glycidyl methacrylate; B4) freeze-drying the dialysate to obtain modified silk protein; C. Preparation of hydrogel for skin transplantation C1) preparing a reaction solution: dissolving tannic acid and zinc chloride in deionized water, then adding modified gelatin and modified silk protein to fully dissolve, and finally adding phenyl (2,4,6-trimethylbenzoyl) lithium phosphate to obtain a mixed solution; C2) The mixed solution obtained in step C1) is irradiated under a blue light ultraviolet lamp of 365-405 nm to form a hydrogel.
2. The use of the hydrogel according to claim 1, characterized in that: The preparation of the modified gelatin in step A satisfies at least any one of the following conditions: The dissolving temperature in step A1) is 40°C; Or, the ratio of gelatin, phosphate buffered saline solution and methacrylic anhydride in step A1) is: For every 1g of gelatin, add 50-100mL of phosphate buffered saline and 0.2-0.8mL of methacrylic anhydride; Or, the reaction in step A1) is performed by stirring the mixture at a water bath temperature; Or, the reaction in step A1) is carried out in a water bath at 40-65° C. for 2-4 hours; Or, in step A2), the amount of PBS dilution solution added is calculated based on the amount of gelatin added, and 100-200 mL of PBS dilution solution is added for every 1 g of gelatin; Or, the pH of the phosphate buffered saline solution in step A1) and step A2) is 7.4; Or, the dialysis device or dialysis bag in step A3) is a dialysis bag; Or, in step A3), the dialysis condition is a molecular weight cut-off of 5-14 kDa, and the dialysis is performed in deionized water at 40-50° C. for 2-3 days.
3. The use of the hydrogel according to claim 2, characterized in that: The preparation of the modified gelatin in step A satisfies at least any one of the following conditions: The ratio of gelatin, phosphate buffered saline solution and methacrylic anhydride in step A1) is: For every 1g of gelatin, add 100mL of phosphate buffered saline and 0.6mL of methacrylic anhydride; Or, the reaction in step A1) is carried out in a water bath at 40° C. for 3 hours; Or, in step A2), the amount of PBS dilution solution added is calculated based on the amount of gelatin added, with 100 mL of PBS dilution solution added for every 1 g of gelatin; Step A3) The dialysis condition is a molecular weight cut-off of 14 kDa, and dialysis is performed in deionized water at 40° C. for 3 days.
4. The use of the hydrogel according to claim 1, characterized in that: The preparation of the modified silk protein in step B satisfies at least any one of the following conditions: Step B1) The concentration of the Na2CO3 aqueous solution is 0.4-1% (w / v); Or, in step B1), the silk cocoons are boiled for 0.5-1 hour under boiling conditions by using a Na2CO3 aqueous solution to remove sericin; Or, in step B2), the ratio of the silk protein, lithium bromide aqueous solution, and glycidyl methacrylate) is as follows: 50-100 mL 9.3 M lithium bromide aqueous solution and 2-8 mL glycidyl methacrylate are added per 10 g of silk protein; Or, the nitrogen protection conditions in step B2) are 100-200rpm, 60-70°C; Or, the reaction time in step B2) is 2-4h; Or, the filtration to remove impurities in step B3) is performed by using a sterile syringe with a 0.22-0.45 μm external filter; Or, the filtration to remove impurities in step B3) is performed by using a sterile syringe with a 0.22 μm or 0.45 μm external filter; Or, the dialysis condition in step B3) is a molecular weight cut-off of 5-14 kDa; Or, during the dialysis in step B3), the dialysis environment temperature is controlled to be lower than 30°C; Alternatively, in step B3), the deionized water dilution of the solution obtained in step B2) is performed to dilute the solution to 5-6 times the volume.
5. The use of the hydrogel according to claim 4, characterized in that: The preparation of the modified silk protein in step B satisfies at least any one of the following conditions: Step B1) The concentration of the Na2CO3 aqueous solution is 0.5% (w / v); Or, in step B1), the silk cocoons are boiled for 1 hour under boiling conditions to remove sericin using the Na2CO3 aqueous solution; Or, the nitrogen protection conditions in step B2) are 400 rpm and 60° C.; Or, the reaction time in step B2) is 3h; Or, in step B2), the ratio of the silk protein, lithium bromide aqueous solution and glycidyl methacrylate is as follows: 75 mL of 9.4 M lithium bromide aqueous solution and 2 mL of glycidyl methacrylate are added per 10 g of silk protein; Or, in step B3), the dialysis condition is a molecular weight cut-off of 14 kDa.
6. The use of the hydrogel according to claim 1, characterized in that: The preparation of the skin transplantation hydrogel in step C satisfies at least any one of the following conditions: Step C1) Prepare the reaction solution according to the following ratio: add 5-10 mg of tannic acid and 2-4 mg of zinc chloride to every 2 ml of deionized water to dissolve, then add 100-200 mg of modified gelatin and 200-300 mg of modified silk protein to fully dissolve, and finally add 20-50 μL of 0.5-1 wt% Lap; Or, in step C2), the irradiation conditions under the blue light ultraviolet lamp are: wavelength 365 or 450nm, irradiation 1-3min.
7. The use of the hydrogel according to claim 6, characterized in that: The preparation of the skin transplantation hydrogel in step C satisfies at least any one of the following conditions: Step C1) Prepare the reaction solution according to the following ratio: add 6 mg of tannic acid and 2 mg of zinc chloride to every 2 ml of deionized water to dissolve, then fully dissolve 200 mg of modified gelatin and 200 mg of modified silk protein, and finally add 50 μL of 0.05 wt% Lap; Or, in step C2), the irradiation conditions under the blue light ultraviolet lamp are: wavelength 405nm, irradiation 1min.
8. The use of the hydrogel according to claim 1, characterized in that: The repairing of the tiny irregular surface or tiny irregular annular surface skin defect is external auditory canal skin grafting in external auditory canal reconstruction.