Rolling manufacturing process of wide titanium plate
Through multiple heating and rotating rolling technology, the problems of lowering the temperature of the titanium slab and single rolling direction are solved, achieving full multi-directional rolling of the titanium slab and improving product quality.
Patent Information
- Application Number
- CN202410845589.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-11
AI Technical Summary
During the rolling process of titanium slab, the temperature decrease makes it unsuitable to continue rolling, and the rolling direction is single and insufficient, which affects product quality.
Using multiple heating and rotating rolling technology, through the cooperation of pressure rollers and brackets, the titanium flat ingots are fully rolled in different directions to avoid temperature reduction and local oxidation. At the same time, oxide scales are removed and separation agents are used to ensure the rolling process. continuity.
It effectively delays the temperature decrease of the titanium slab, achieves multi-directional and sufficient rolling, improves product quality and production efficiency, and avoids the problems of local oxidation and uneven rolling.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material processing, and in particular to a rolling manufacturing process for a wide titanium plate. Background Art
[0002] Due to the excellent comprehensive properties of titanium and titanium alloy materials such as low density, high specific strength, corrosion resistance, and good stability of organizational properties, titanium and titanium alloy materials have developed rapidly in recent decades. my country's titanium industry began in the 1960s with the requirements of national defense and military industry. After 50 years of development, it has achieved great results. At present, titanium processing materials have developed rapidly in the fields of aviation, aerospace, shipbuilding, metallurgy, chemical industry, equipment, medical treatment, pharmaceuticals, marine engineering, sports and leisure. my country is rich in titanium resources and its reserves are among the highest in the world. It has now become a titanium power with a complete industrial system and production capacity in the world. Its production and consumption rank first in the world. Titanium and titanium alloys are processed into plates, strips, foils, tubes, rods, wires, forgings, castings and composite materials. Among all titanium alloy processing materials, the output of titanium plates and strips is close to 50%. Titanium plates and strips are widely used, mainly used to make aircraft engine compressor parts, followed by rockets, missiles and high-speed aircraft structural parts.
[0003] The temperature of the titanium slab will continue to decrease during rolling. After rolling to a certain extent and for a period of time, the temperature of the titanium slab will decrease too much and become unsuitable for further rolling. Usually, when rolling the titanium slab, the titanium slab must be rotated to be rolled in different directions, and the rolling direction is usually single, resulting in insufficient rolling. Summary of the invention
[0004] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a rolling manufacturing process for wide-width titanium plates.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A rolling manufacturing process for a wide titanium plate is designed, the manufacturing process comprising:
[0007] S1: using a titanium slab as a raw material, wherein the original thickness of the titanium slab is 100-300 mm;
[0008] S2: heating the titanium slab for the first time;
[0009] S3: After the first heating is completed, the titanium slab is rolled by the pressing roller, and then the motor is started, and the pressing roller is rotated 5-15 degrees by the support of the bracket, and then rolling is performed, and the pressing roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until a titanium slab with a thickness of less than 50% of the original thickness of the titanium slab and a length that meets the target width requirement is formed;
[0010] S4: performing a second heating on the titanium ingot;
[0011] S5: heating the pressure roller;
[0012] S6: After the second heating is completed, the titanium slab is rolled by the pressing roller, and then the motor is started, and the pressing roller is rotated 5-15 degrees by the support of the bracket, and then rolling is performed, and the pressing roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until a titanium slab with a thickness of less than 20% of the original thickness of the titanium slab and a length that meets the target width requirement is formed;
[0013] S7: sequentially cooling the titanium slab after the first round of rolling;
[0014] S8: removing the oxide scale on the upper and lower surfaces of the titanium plate and cutting off the defects that affect the re-rolling;
[0015] S9: heating the titanium slab after the surface treatment for a third time;
[0016] S10: applying a separating agent on a supporting block supporting the titanium slab;
[0017] S11: heating the supporting block supporting the titanium slab.
[0018] S12: After the third heating is completed, the titanium slab is rolled in one direction by a pressure roller, and then the motor is started, and the pressure roller is rotated 60-180 degrees by the support of the bracket, and then rolling is performed, and the pressure roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until the thickness of the titanium slab is 1.0-2.0% of the original thickness of the titanium slab.
[0019] Preferably, the step S5 further includes: heating a supporting block supporting the titanium slab.
[0020] Preferably, the step S2 further includes: heating the pressure roller.
[0021] Preferably, the step S10 further includes: heating the pressure roller.
[0022] Preferably, the S10 further includes:
[0023] T1: Grind the roller with sandpaper to remove the attached oxides;
[0024] T2: Clean and polish the oxide attached to the supporting block supporting the titanium slab.
[0025] Preferably, the pressure roller is detachably connected to the bracket, and the pressure roller can be installed on the bracket after heating the pressure roller.
[0026] The invention proposes a rolling manufacturing process for a wide-width titanium plate, which has the beneficial effect of: heating the supporting block supporting the titanium slab through step S11. After rolling to a certain extent and for a period of time, the temperature of the titanium slab will not drop too much to make it unsuitable for further rolling. Step S5: heating the pressure roller can also avoid local oxidation when the low-temperature pressure roller contacts the titanium slab. The titanium flat ingot is rolled by the pressure roller, and then the motor is started. The pressure roller is rotated by a certain angle through the support of the bracket, and then rolling is carried out, and it rotates one circle in turn. This process does not require the titanium slab to be rotated. The motor can be used to roll in different directions, and the rolling direction is rich and the rolling is sufficient. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0028] A rolling manufacturing process for a wide titanium plate, the manufacturing process comprising:
[0029] S1: Titanium ingot is used as raw material, and the original thickness of the titanium ingot is 100-300mm; the titanium ingot can be round or rectangular, and the selected material has rich shapes.
[0030] S2: The titanium slab is heated for the first time to facilitate rolling by the rollers. It also includes: heating the rollers to prevent the low-temperature rollers from contacting the titanium slab and causing local oxidation of the titanium slab.
[0031] S3: After the first heating is completed, the titanium slab is rolled by the roller, and then the motor is started. The roller is rotated 5-15° by the support of the bracket, and then rolling is performed. The roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly. Due to the large thickness of the titanium slab, it needs to be rolled repeatedly. Until a titanium slab with a thickness of less than 50% of the original thickness of the titanium slab and a length that meets the target width requirement is formed; this process does not require the titanium slab to be rotated, and the motor can be used to roll in different directions, and the rolling direction is rich and the rolling is sufficient;
[0032] S4: heating the titanium ingot for the second time; heating multiple times to avoid single heating, which will cause the heat to dissipate quickly and affect the rolling effect, so as to facilitate rolling by the roller;
[0033] S5: heating the pressing rollers; this will also prevent the low-temperature pressing rollers from contacting the titanium slabs, causing local oxidation of the titanium slabs. It also includes: heating the support blocks that support the titanium slabs; after rolling to a certain extent and for a period of time, the temperature of the titanium slabs will not drop too much to make it unsuitable for further rolling;
[0034] S6: After the second heating is completed, the titanium slab is rolled by the roller, and then the motor is started. The roller is rotated 5-15° by the support of the bracket, and then rolling is performed. The roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly. Due to the large thickness of the titanium slab, it needs to be rolled repeatedly. Until a titanium slab with a thickness of less than 20% of the original thickness of the titanium slab and a length that meets the target width requirement is formed; this process does not require the titanium slab to be rotated, and the motor can be used to roll in different directions, and the rolling direction is rich and the rolling is sufficient;
[0035] S7: cooling the titanium slabs after the first round of rolling in sequence; the cooling may be performed by spraying cold air onto the titanium slabs.
[0036] S8: Remove the oxide scale on the upper and lower surfaces of the titanium slab and cut off the defects that affect the re-rolling; remove the oxide scale by sandpaper grinding, and grind the titanium slab flat.
[0037] S9: heating the titanium slab after surface treatment for the third time; multiple heating to avoid single heating, which causes rapid heat dissipation and affects the rolling effect, making it easier for the roller to roll it;
[0038] S10: Apply a separating agent on the supporting block supporting the titanium slab to facilitate quick removal of the titanium slab. It also includes: heating the pressing roller to prevent the low-temperature pressing roller from contacting the titanium slab, causing local oxidation of the titanium slab.
[0039] T1: Grind the rollers with sandpaper to remove the attached oxides; prepare for the third rolling so that the titanium slab will not be rolled unevenly.
[0040] T2: Clean and polish the oxides attached to the supporting block supporting the titanium slab; prepare for the third rolling so that when the titanium slab is rolled, there will be no oxides on the surface of the titanium slab that contacts the supporting block.
[0041] S11: heating the support block supporting the titanium slab. After rolling to a certain extent and for a period of time, the temperature of the titanium slab will not drop too much to make it unsuitable for further rolling;
[0042] S12: After the third heating is completed, the titanium slab is rolled in one direction by the pressure roller, and then the motor is started. The pressure roller is rotated 60-180° by the support of the bracket, and then rolling is performed. The roller rotates one circle in turn, and the above operation is repeated repeatedly. Since the thickness of the titanium slab is large, it needs to be rolled repeatedly. The thickness of the titanium slab is 1.0-2.0% of the original thickness of the titanium slab. This process does not require the rotation of the titanium slab, and the motor can be used to roll in different directions, and the rolling direction is rich and the rolling is sufficient.
[0043] The pressure roller is detachably connected to the bracket, and the pressure roller can be installed on the bracket after heating the pressure roller. The pressure roller can be installed by heating the pressure roller first and then installing it.
[0044] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A rolling manufacturing process for wide titanium plates, characterized in that: The manufacturing process comprises: S1: using a titanium slab as a raw material, wherein the original thickness of the titanium slab is 100-300 mm; S2: heating the titanium slab for the first time; S3: After the first heating is completed, the titanium slab is rolled by the pressing roller, and then the motor is started, and the pressing roller is rotated 5-15 degrees by the support of the bracket, and then rolling is performed, and the pressing roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until a titanium slab with a thickness of less than 50% of the original thickness of the titanium slab and a length that meets the target width requirement is formed; S4: performing a second heating on the titanium ingot; S5: heating the pressure roller; S6: After the second heating is completed, the titanium slab is rolled by the pressing roller, and then the motor is started, and the pressing roller is rotated 5-15 degrees by the support of the bracket, and then rolling is performed, and the pressing roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until a titanium slab with a thickness of less than 20% of the original thickness of the titanium slab and a length that meets the target width requirement is formed; S7: sequentially cooling the titanium slab after the first round of rolling; S8: removing the oxide scale on the upper and lower surfaces of the titanium plate and cutting off the defects that affect the re-rolling; S9: heating the titanium slab after the surface treatment for a third time; S10: applying a separating agent on a supporting block supporting the titanium slab; S11: heating the supporting block supporting the titanium slab. S12: After the third heating is completed, the titanium slab is rolled in one direction by a pressure roller, and then the motor is started, and the pressure roller is rotated 60-180 degrees by the support of the bracket, and then rolling is performed, and the pressure roller is rotated for one circle in turn, and the above rolling operation is repeated repeatedly until the thickness of the titanium slab is 1.0-2.0% of the original thickness of the titanium slab.
2. The rolling manufacturing process of a wide titanium plate according to claim 1 is characterized in that: The step S5 further includes: heating a supporting block supporting the titanium slab.
3. The rolling manufacturing process of a wide titanium plate according to claim 1, characterized in that: The step S2 further includes: heating the pressure roller.
4. The rolling manufacturing process of a wide titanium plate according to claim 1 is characterized in that: The step S10 further includes: heating the pressure roller.
5. The rolling manufacturing process of a wide titanium plate according to claim 1 is characterized in that: The S10 further includes: T1: Grind the roller with sandpaper to remove the attached oxides; T2: Clean and polish the oxide attached to the supporting block supporting the titanium slab.
6. The rolling manufacturing process of a wide titanium plate according to claim 1, characterized in that: The pressing roller is detachably connected to the bracket, and the pressing roller can be installed on the bracket after being heated.
Citation Information
Patent Citations
Thick plate broadening mode control method and device
CN112427462A
Rolling method of wide and thick plate rolling mill
CN114632817A
Method for preparing high-strength weak-texture magnesium alloy through multi-directional rolling
CN116213456A
Production of austenitic stainless steel plate for thermal neutron shielding
JP1996253814A