Welding method for silicon carbide ceramic and metal material
Through activation treatment and vacuum welding technology, the problem of weak connection between silicon carbide ceramics and metal welding under high temperature conditions is solved, a high tensile strength welding effect is achieved, and the overall performance and reliability of the product are improved.
Patent Information
- Application Number
- CN202411132999.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-10-11
AI Technical Summary
The existing technology is difficult to weld silicon carbide ceramics and metal together under high temperature conditions, and cannot achieve high tensile strength, resulting in weak connections and prone to falling.
By activating the silicon carbide material, prepare an activated slurry and apply it on the area to be welded. After baking and activation, AgCu solder is applied, and welded in a vacuum environment, applying uniform pressure to improve the welding strength.
It effectively improves the tensile strength of silicon carbide and metal, solves the problem of weak connection, avoids falling, and improves the overall performance and reliability of the product.
Smart Images

Figure CN118752108A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of material science and engineering, and in particular to a welding method for silicon carbide ceramics and metal materials. Background Art
[0002] Silicon carbide ceramics are an advanced ceramic material mainly composed of silicon and carbon elements. Silicon carbide has excellent high-temperature stability, high thermal conductivity, low thermal expansion coefficient, low thermal deformation, high specific stiffness and excellent thermal uniformity. It is not easy to bend or deform after long-term use. In some industrial components, it is necessary to work under high temperature conditions such as above 300°C for a long time. The thermal conductivity of conventional ceramics cannot be applied, so silicon carbide ceramics can be used.
[0003] However, some components require silicon carbide and metal to be welded together and achieve higher tensile strength. Many conventional metallization methods such as thin film metallization, thick film metallization, and laser metallization cannot solve this problem. Therefore, it is necessary to design a method to weld silicon carbide and metal together and achieve the tensile strength requirements. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, an object of the present invention is to provide a welding method of silicon carbide ceramics and metal materials to solve one or more problems in the prior art.
[0005] To achieve the above object, the technical solution of the present invention is as follows:
[0006] A method for welding silicon carbide ceramic and metal material, comprising the following steps:
[0007] Activation treatment of silicon carbide materials;
[0008] Silicon carbide material coated with solder for welding preparation;
[0009] Vacuum welding.
[0010] Furthermore, the activation treatment of the silicon carbide material comprises the following steps:
[0011] preparing an activated slurry;
[0012] Apply activation slurry to the area to be welded;
[0013] Bake to activate the silicon carbide material.
[0014] Furthermore, the preparation of the activated slurry comprises the following steps:
[0015] Molybdenum powder ball milling;
[0016] Preparation of terpineol;
[0017] The active layer material is mixed with pinene alcohol.
[0018] Furthermore, when the molybdenum powder is ball-milled, the ratio of balls to molybdenum powder is 1:1, the ball-milling speed is 240-260 r / min, and the ball-milling time is 72-73 hours.
[0019] Furthermore, the preparation of terpineol is that terpineol and ethyl cellulose are dissolved in a ratio of 1:9, the dissolution temperature is 65° C. to 70° C., and the dissolution time is 8 to 8.5 hours.
[0020] Furthermore, when the active layer material is mixed with pine oil, the weight ratio of the active layer material to pine oil is 4:1, and the mixing time is 24 to 24.5 hours; the active layer material includes molybdenum, manganese, titanium and tin, and the corresponding ratio is 5:2:2:1.
[0021] Furthermore, the thickness of the activated slurry applied to the area to be welded is 5um to 10um.
[0022] Furthermore, the baking temperature of the baking activated silicon carbide material is 115-125° C., and the baking time is 50-70 minutes.
[0023] Furthermore, the silicon carbide material is coated with solder for soldering preparation, the solder is AgCu solder, and the coating thickness is 30um to 50um.
[0024] Furthermore, during the vacuum welding, a pressure of 1 to 2 kg is uniformly applied to the weld.
[0025] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0026] The present invention improves the tensile strength by welding metal and silicon carbide together through a welding method, effectively solves the problem that the traditional silicon carbide metallization has low permeability and cannot penetrate into silicon carbide, resulting in a weak connection between silicon carbide and metal, avoids the phenomenon of silicon carbide falling off when the metal touches lightly, and improves the overall performance and reliability of the product. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A schematic diagram of a welding process of silicon carbide ceramic and metal material according to an embodiment of the present invention is shown.
[0028] Figure 2 A structural schematic diagram of welding of silicon carbide ceramic and metal material according to an embodiment of the present invention is shown.
[0029] Markings in the accompanying drawings: 1, metal; 2, solder; 3, active layer; 4, silicon carbide. DETAILED DESCRIPTION
[0030] In order to make the purpose, technical scheme and advantages of the present invention clearer, the following is a further detailed description of a welding method for silicon carbide ceramics and metal materials proposed by the present invention in combination with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will be clearer. It should be noted that the accompanying drawings are in a very simplified form and use non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. In order to make the purpose, features and advantages of the present invention more obvious and easy to understand, please refer to the accompanying drawings. It should be noted that the structure, proportion, size, etc. illustrated in the drawings of this specification are only used to match the content disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no technical substantive significance. Any modification of the structure, change in the proportional relationship or adjustment of the size, without affecting the effect that the present invention can produce and the purpose that can be achieved, should still fall within the scope of the technical content disclosed by the present invention.
[0031] See also Figure 1 and Figure 2 The welding method of silicon carbide ceramic and metal material of this embodiment comprises the following steps:
[0032] Step 1: Activation treatment of silicon carbide 4 material:
[0033] Step 1.1: Preparation of activation slurry:
[0034] Step 1.1.1: Ball milling of molybdenum powder:
[0035] Select a suitable matrix material, preferably, in this embodiment, molybdenum powder is included, and these materials will be used as the basis for making the activated slurry. The ratio of balls to molybdenum powder during ball milling is 1:1. Put the molybdenum powder into a ball mill for ball milling. During the ball milling process, the powder is subjected to impact, shear, friction, compression and other forces, and large particles will be broken into small particles, and small particles will be broken into smaller particles or debris. By controlling the ball milling parameters such as the speed of the ball mill, the ball milling time and other parameters, in this embodiment, the ball mill speed is 240-260r / min. The ball milling time is 72-73 hours, and molybdenum powder with uniform particle size and reasonable distribution can be obtained.
[0036] Step 1.1.2: Preparation of terpineol:
[0037] High-quality terpineol products can be prepared by accurate raw material ratio, selection of catalysts and emulsifiers, and strict control of reaction conditions. In this embodiment, the preparation of terpineol is that terpineol and ethyl cellulose are dissolved in a ratio of 1:9, the dissolution temperature is 65°C to 70°C, and the dissolution time is 8 to 8.5 hours.
[0038] Step 1.1.3: Active layer 3 material is mixed with pinene alcohol.
[0039] The active layer 3 material includes molybdenum, manganese, titanium and tin, which are put into a mixer in a corresponding ratio of 5:2:2:1, and at the same time, the prepared pineol is added to the mixer in an amount according to a weight ratio of the active layer 3 material to pineol of 4:1. The mixing time of the mixer is set to 24 to 24.5 hours, so that the above-mentioned active layer 3 material is fully dissolved to form an activated slurry.
[0040] Step 1.2: Apply activation slurry to the area to be welded:
[0041] The prepared activation slurry is evenly coated on the area to be welded on the silicon carbide 4 , wherein the thickness of the activation slurry is 5 um to 10 um, to form an active layer 3 .
[0042] Step 1.3: Bake to activate the SiC 4 material.
[0043] In order to improve the performance of the silicon carbide 4, especially in applications that require it to have good dispersibility, stability and high-temperature performance, it is necessary to bake the silicon carbide 4 coated with the activated slurry. The baking temperature for baking the activated silicon carbide 4 material is 115-125°C and the baking time is 50-70 minutes.
[0044] Step 2: Silicon carbide 4 material coated with solder 2 preparation for welding:
[0045] After baking, solder 2 is coated on the surface of the active layer 3 for preparation for welding. The solder 2 is AgCu solder, which is a silver alloy with copper as the main alloy element. Nickel, beryllium, lithium, vanadium and other elements are usually added to improve the performance. It has good mechanical properties, wear resistance and resistance to fusion welding. It also has good conductivity, fluidity and wettability. The thickness of the solder 2 is 30um to 50um.
[0046] Step 3: Vacuum welding.
[0047] The metal 1 is butted with the solder 2 and welded in a vacuum environment. Under vacuum conditions, the gas molecules are scarce during the welding process, which reduces the interference of the gas on the joint during the welding process. At the same time, the oxides, inclusions and pores formed on the surface of the welding material will be effectively removed, thereby reducing the porosity inside the joint and ensuring the high purity of the welded joint. At the same time, the crystal particles of the welded joint are fine and evenly distributed, so that the strength of the welded joint is high. When performing vacuum welding, a pressure of 1 to 2 kg is evenly applied to the weld. By evenly applying pressure, the diffusion and chemical reaction of the metal 1 can be promoted, which is conducive to the merging and formation of the weld, making the welding quality more uniform and stable.
[0048] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0049] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for welding silicon carbide ceramics and metal materials, Features The following steps are involved: Activation treatment of silicon carbide materials; Silicon carbide material coated with solder for welding preparation; Vacuum welding.
2. A method for welding silicon carbide ceramic and metal material as claimed in claim 1, Features: The activation treatment of the silicon carbide material comprises the following steps: preparing an activated slurry; Apply activation slurry to the area to be welded; Bake to activate the silicon carbide material.
3. A method for welding silicon carbide ceramic and metal material as claimed in claim 2, Features The preparation of the activated slurry comprises the following steps: Molybdenum powder ball milling; Preparation of terpineol; The active layer material is mixed with pinene alcohol.
4. A method for welding silicon carbide ceramic and metal material as claimed in claim 3, Features: When the molybdenum powder is ball-milled, the ratio of balls to molybdenum powder is 1:1, the ball-milling speed is 240-260 r / min, and the ball-milling time is 72-73 hours.
5. A method for welding silicon carbide ceramic and metal material as claimed in claim 4, Features: The preparation of terpineol is that terpineol and ethyl cellulose are dissolved in a ratio of 1:9, the dissolution temperature is 65° C. to 70° C., and the dissolution time is 8 to 8.5 hours.
6. A method for welding silicon carbide ceramic and metal material as claimed in claim 5, Features: When the active layer material is mixed with pine oil, the weight ratio of the active layer material to pine oil is 4:1, and the mixing time is 24 to 24.5 hours; the active layer material includes molybdenum, manganese, titanium and tin, and the corresponding ratio is 5:2:2:
1.
7. A method for welding silicon carbide ceramic and metal material as claimed in claim 2, Features: The thickness of the activated slurry coated on the welded area is 5um to 10um.
8. A method for welding silicon carbide ceramic and metal material as claimed in claim 7, Features: The baking temperature of the baking activated silicon carbide material is 115-125° C., and the baking time is 50-70 minutes.
9. A method for welding silicon carbide ceramic and metal material as claimed in claim 1, Features: The silicon carbide material is coated with solder for welding preparation, the solder is AgCu solder, and the coating thickness is 30um-50um.
10. A method for welding silicon carbide ceramic and metal material as claimed in claim 1, Features: During the vacuum welding, a pressure of 1 to 2 kg is uniformly applied to the weld.