Copper steel brazing coaxial injector forming method based on additive manufacturing process

Through the copper-steel brazed coaxial injector forming method based on the additive manufacturing process, the problems of complicated production process and poor material quality of the liquid rocket engine injector are solved, and efficient and stable injector forming and The ablation resistance of the combustion chamber reduces costs and improves reliability.

CN118752176APending Publication Date: 2024-10-11XIAN SPACE ENGINE CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410377568.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The production process of the existing liquid rocket engine coaxial injector is complex, long cycle, and high cost, and the additively manufactured copper alloy material cannot meet the requirements of the combustion chamber in a high-temperature and high-pressure environment, resulting in poor injector quality and ablation problem.

Method used

Using a copper-steel brazed coaxial injector forming method based on additive manufacturing processes, the stainless steel main nozzle and Copper alloy partition nozzle enables efficient forming and stable connection of complex structures.

Benefits of technology

It improves the processing efficiency and quality of the injector and reduces the production cost. The additive manufacturing injector has zoned combustion stability, suppresses high-frequency combustion instability and ablation problems, and improves the ablation resistance and reliability of the product. sex.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752176A_ABST
    Figure CN118752176A_ABST
Patent Text Reader

Abstract

The invention relates to a copper steel brazing coaxial type injector forming method based on an additive manufacturing process, and belongs to the technical field of liquid rocket engine manufacturing. A traditional brazing coaxial type injector partition plate nozzle is divided into an upper part and a lower part, the upper half part, the middle bottom, the inner bottom and the main nozzle are integrally formed through the additive manufacturing technology, the main injector structural part is obtained and made of stainless steel, and the method is simple in machining process and high in production efficiency. And meanwhile, in order to improve the ablation resistance of the partition plate nozzle in a combustion chamber, the lower half part of the partition plate nozzle adopts a copper-copper brazed part to form a brazed partition plate nozzle. And the two are connected through brazing. The problems that a traditional tube plate type brazing injector with hundreds of parts is long in machining period and complex in machining process can be solved, the ablation resistance of a partition plate nozzle of the injector in unstable combustion can be improved, the manufacturing cost can be reduced, and the product reliability can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for forming a copper-steel brazing coaxial injector based on an additive manufacturing process, belonging to the technical field of liquid rocket engine manufacturing, and in particular to the field of combustion component injector manufacturing. Background Art

[0002] The thrust chamber injector is a key combustion component that realizes the mixing, collision, atomization and combustion of the two propellants of the liquid rocket engine to form the main power. The coaxial injector is a common one. The coaxial injector of the liquid oxygen-kerosene engine in service is composed of a machined inner bottom and a middle bottom with milled grooves. Hundreds of coaxial brazed nozzles are installed between the two bottoms, which are brazed into a whole to form an internal cavity that is not connected to each other. The disadvantages of this method are: the middle bottom and the inner bottom are generally forgings, involving forging, heat treatment, machining, and electrospark machining. The middle bottom and the main nozzle are made of stainless steel, and the partition nozzle is made of copper alloy; the nozzle is generally composed of two types of nozzles, the side area and the center. A brazed nozzle machine has at least 4 types of nozzles. After the processing of the 4 nozzles is completed, liquid flow needs to be carried out and repaired according to the liquid flow results and assembled separately; the assembly of the injector requires trial assembly, drilling, and electroplating. The production involves many professions and complex processes, with a long production cycle and high manufacturing costs.

[0003] In view of the above shortcomings, the process scheme of using additive manufacturing to integrally form the injector is proposed. This process method has a simple processing flow, short cycle and low manufacturing cost. However, the internal quality density of the product using copper alloy materials for additive manufacturing is insufficient, the technology is difficult, and the manufacturing cost is high; the baffle nozzle of the additive manufacturing process using stainless steel injector materials cannot meet the high temperature and high pressure environment in the combustion chamber and ablation occurs. Therefore, the injector currently formed by additive manufacturing is a stainless steel injector without a baffle nozzle for partitioned combustion. Summary of the invention

[0004] The technical problem solved by the present invention is: to overcome the shortcomings of the prior art, to propose a copper-steel brazing coaxial injector forming method based on additive manufacturing process, and to improve the processing efficiency and processing quality of injectors with complex structures.

[0005] The technical solution of the present invention is:

[0006] The present invention discloses a method for forming a copper-steel brazing coaxial injector based on an additive manufacturing process, comprising:

[0007] Carry out 3D modeling of the main nozzle structure of the injector to obtain the main nozzle structure model;

[0008] Optimizing the main nozzle structure model to obtain the main nozzle model;

[0009] According to the main nozzle model, laser forming processing is performed to obtain a main nozzle structure blank;

[0010] The main nozzle structure blank is subjected to chemical finishing treatment and a liquid flow test is performed for verification; after the liquid flow test verification meets the requirements, mechanical processing is performed;

[0011] The outlet end of the main nozzle structural part blank is machined to obtain the brazing butt surface of the main nozzle structural part;

[0012] Performing plating treatment on the brazing butt joint surface of the main nozzle structural component;

[0013] Pre-setting brazing material on the brazing butt joint surface of the main nozzle structural part after the plating treatment to obtain the main nozzle structural part;

[0014] Processing and brazing the brazed baffle nozzle to obtain the brazed baffle nozzle;

[0015] The brazing partition nozzle and the main nozzle structural parts are preassembled and placed in a brazing furnace for brazing to obtain a brazing injector.

[0016] Furthermore, in the above forming method, the brazing injector comprises: a main nozzle structure and a brazing partition nozzle, wherein:

[0017] The main nozzle structure comprises a nozzle and a main body structure; the main body structure is a cylindrical structure, and the cylindrical structure comprises a first end head, a middle part and a second end head which are coaxially connected in sequence; the middle part is composed of two thin plates with a hollow interlayer, and the inner thin plate is provided with a through hole; the inner layer of the first end head is provided with a fluid channel;

[0018] The nozzle is inserted between the two thin plates in the middle part, and the axis of the nozzle is parallel to the axis of the cylindrical structure; one end of the nozzle is flush with the outer surface of the thin plate on one side connected to the first end, and the other end of the nozzle passes through the middle part;

[0019] The nozzle comprises a plurality of main nozzles and a plurality of upper parts of baffle nozzles; wherein the upper parts of the baffle nozzles are coaxially connected to the brazed baffle nozzle; the plurality of main nozzles and the upper parts of the baffle nozzles are arranged in parallel; the brazed baffle nozzle comprises an inner shell and an outer shell, wherein the inner shell is placed inside the outer shell and connected to the outer shell surface.

[0020] Furthermore, in the above forming method, the main nozzle structure is made of stainless steel and formed by additive manufacturing; the brazed partition nozzle is made of copper alloy.

[0021] Furthermore, in the above forming method, the structural model is optimized, specifically: a transition chamfer area is added at the connection between the two thin plates in the middle part of the main nozzle structure and the nozzle, and the angle θ between the chamfer slope and the injection surface is less than 45°.

[0022] Furthermore, in the above forming method, laser forming is performed according to the main nozzle model to obtain a main nozzle structure blank, and the specific method is:

[0023] According to the main nozzle model, a laser selective melting forming process is adopted to form a main nozzle structure;

[0024] The formed main nozzle structure is subjected to stabilization heat treatment, the substrate is wire-cut, and excess powder and support are removed to obtain a main nozzle structure blank.

[0025] Furthermore, in the above forming method, the brazing baffle nozzle is processed and brazed to obtain the brazing baffle nozzle, and the specific method is:

[0026] Processing and pre-assembling the inner shell and the outer shell to obtain an assembly;

[0027] Conduct a liquid flow test on the assembly and obtain the test results;

[0028] According to the test results, the inner shell and the outer shell are further processed until they meet the requirements, thereby obtaining the inner shell and the outer shell after the deep processing;

[0029] Plating the inner shell after deep processing to obtain a plated inner shell;

[0030] The plated inner shell is pre-filled with brazing material and connected to the outer shell by brazing to obtain a preliminary sample of a brazed partition nozzle;

[0031] The inlet end of the brazed baffle nozzle prototype is machined to form a brazing butt surface to obtain a brazed baffle nozzle.

[0032] Furthermore, in the above forming method, two annular channels I are formed at the pre-assembly connection of the inner shell and the outer shell, with a rectangular cross-section and a length and width of L1 and L2 respectively, for pre-setting brazing material; wherein L1 = 0.8-0.9 mm, L2 = 0.8-0.9 mm.

[0033] Furthermore, in the above forming method, the inner shell after deep processing is plated, specifically: after the outer surface of the inner shell is pickled and degreased, nickel and manganese are plated on the surface to be brazed by chemical electroplating, the nickel layer thickness is 1 to 2 μm, the manganese layer thickness is 5 to 10 μm, and the inner surface of the outer shell is pickled and degreased.

[0034] Furthermore, in the above forming method, the brazing joint surface of the main nozzle structural component is plated, specifically: the surface of the main nozzle structural component to be brazed is pickled and degreased, and then nickel is plated by chemical electroplating, and the thickness of the nickel layer is 5 to 10 μm.

[0035] Furthermore, in the above-mentioned forming method, the brazing baffle nozzle and the main nozzle structural member are pre-assembled, specifically: the brazing baffle nozzle is sleeved on the inner side of the main nozzle structural member, and a first annular channel, a second annular channel, a first brazing surface and a second brazing surface are formed between the outer wall of the brazing baffle nozzle and the inner wall of the main nozzle structural member; the first annular channel has a rectangular cross-section, and a length and width of 0.28 to 0.35 mm and 2.05 to 2.1 mm, respectively, and the second annular channel has a rectangular cross-section, and a width and length of 0.55 to 0.58 mm and 0.5 to 0.55 mm, respectively; the first annular channel and the second annular channel are used for pre-setting brazing material; the fitting clearance between the first brazing surface and the second brazing surface is 0.02 mm to 0.35 mm.

[0036] Furthermore, in the above-mentioned forming method, the annular channel I is pre-set with a filamentary annular solder Q1 with a specification of φ0.7~0.9mm, 1~2 circles, and fixed by riveting with sample punching points; the first annular channel is pre-set with 1~2 solders Q2 with a size of δ0.2~0.3mm, and the second annular channel is pre-set with 1~2 solders Q2 with a size of δ0.1~0.2mm, and riveting is performed for positioning by sample punching points; the melting point of the solder Q1 is 80~100°C higher than that of the solder Q2. After the brazing assembly formed by the solder Q1 is brazed, it is brazed with the solder ring Q2.

[0037] Furthermore, in the above forming method, the brazing methods are gas shielded brazing and vacuum brazing, wherein the assembly formed by the brazing material Q1 is brazed by gas shielded brazing, and the brazing temperature is 940-970°C; the assembly formed by the brazing material Q2 is brazed by vacuum brazing, and the brazing temperature is 850-870°C.

[0038] The advantages of the present invention compared with the prior art are:

[0039] 1. The present invention effectively solves the problem that copper and steel dissimilar materials cannot be connected by additive manufacturing, improves the processing efficiency and processing quality of complex structure injectors, and reduces production costs.

[0040] 2. The present invention realizes zoned combustion of additively manufactured injectors, which can suppress the instability of high-frequency combustion, solve the problem of injector stable combustion nozzle ablation and combustion unevenness.

[0041] 3. The present invention can not only solve the problems of long processing cycle and complicated processing flow of traditional tube-to-sheet brazing injectors with hundreds of parts, but also improve the ablation resistance of the injector baffle nozzle in unstable combustion, reduce manufacturing costs and improve product reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 It is a schematic diagram of the structure of the injector of the present invention;

[0043] Figure 2 This is a diagram of a brazed baffle nozzle of the present invention;

[0044] Figure 3 This is a schematic diagram of the structure of the brazing butt joint surface of the injector of the present invention;

[0045] Figure 4 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0046] The present invention adopts additive manufacturing technology to integrally form the bottom, inner bottom, a large number of main nozzles and the upper half of the baffle nozzle in the traditional brazing scheme. The material is stainless steel. After forming, the nozzle outlet end face is flat, and the baffle nozzle brazing interface is formed by mechanical processing; the number of brazed baffle nozzles is small, and a gas-shielded brazing scheme is used for the inner and outer shells. After the nozzle is formed, the brazing interface is formed by mechanical processing; the two are vacuum brazed to form an injector.

[0047] The present invention discloses a method for forming a copper-steel brazing coaxial injector based on an additive manufacturing process, comprising:

[0048] Carry out 3D modeling of the main nozzle structure of the injector to obtain the main nozzle structure model;

[0049] Optimizing the main nozzle structure model to obtain the main nozzle model;

[0050] According to the main nozzle model, laser forming processing is performed to obtain a main nozzle structure blank;

[0051] The main nozzle structure blank is subjected to chemical finishing treatment and a liquid flow test is performed for verification; after the liquid flow test verification meets the requirements, mechanical processing is performed;

[0052] The outlet end of the main nozzle structural part blank is machined to obtain the brazing butt surface of the main nozzle structural part;

[0053] Performing plating treatment on the brazing butt joint surface of the main nozzle structural component;

[0054] Pre-setting brazing material on the brazing butt joint surface of the main nozzle structural part after the plating treatment to obtain the main nozzle structural part;

[0055] Processing and brazing the brazed baffle nozzle to obtain the brazed baffle nozzle;

[0056] The brazing partition nozzle and the main nozzle structural parts are preassembled and placed in a brazing furnace for brazing to obtain a brazing injector.

[0057] Preferably, the brazing injector comprises: a main nozzle structure 1 and a brazing partition nozzle 2, wherein:

[0058] The main nozzle structure 1 includes a nozzle and a main structure 5; the main structure 5 is a cylindrical structure, and the cylindrical structure includes a first end head, a middle part and a second end head which are coaxially connected in sequence; the middle part is composed of two thin plates with a hollow interlayer, and the inner thin plate is provided with a through hole; the inner layer of the first end head is provided with a fluid channel;

[0059] The nozzle is inserted between the two thin plates in the middle part, and the axis of the nozzle is parallel to the axis of the cylindrical structure; one end of the nozzle is flush with the outer surface of the thin plate on one side connected to the first end, and the other end of the nozzle passes through the middle part;

[0060] The nozzle comprises a plurality of main nozzles 3 and a plurality of baffle nozzle upper parts 4; wherein the baffle nozzle upper part 4 is coaxially connected with the brazed baffle nozzle; the plurality of main nozzles 3 and the plurality of baffle nozzle upper parts 4 are arranged in parallel; Figure 2 As shown, the brazed baffle nozzle 2 comprises an inner shell 6 and an outer shell 7 , wherein the inner shell 6 is disposed inside the outer shell 7 and is surface-connected to the outer shell 7 .

[0061] Preferably, the main nozzle structure 1 is made of stainless steel and formed by additive manufacturing; the brazed partition nozzle 2 is made of copper alloy.

[0062] Preferably, the structural model is optimized, specifically: a transition chamfered area is added at the connection between the two thin plates in the middle part of the main nozzle structure 1 and the nozzle, and the angle θ between the chamfered slope and the injection surface is less than 45°, such as Figure 1 shown.

[0063] Preferably, laser forming is performed according to the main nozzle model to obtain a main nozzle structure blank, and the specific method is:

[0064] According to the main nozzle model, the laser selective melting forming process is used to form the main nozzle structure; the product during forming is Figure 1 The position shown is rotated 180°; during forming, the first end is at the top and the main body axis is parallel to the substrate;

[0065] The formed main nozzle structure is subjected to stabilization heat treatment, the substrate is wire-cut, and excess powder and support are removed to obtain a main nozzle structure blank.

[0066] Preferably, the brazing baffle nozzle is processed and brazed to obtain the brazing baffle nozzle, and the specific method is as follows:

[0067] Processing and pre-assembling the inner shell and the outer shell to obtain an assembly;

[0068] Conduct a liquid flow test on the assembly and obtain the test results;

[0069] According to the test results, the inner shell and the outer shell are further processed until they meet the requirements, thereby obtaining the inner shell and the outer shell after the deep processing;

[0070] Plating the inner shell after deep processing to obtain a plated inner shell;

[0071] The plated inner shell is pre-filled with brazing material and connected to the outer shell by brazing to obtain a preliminary sample of a brazed partition nozzle;

[0072] The inlet end of the brazed baffle nozzle prototype is machined to form a brazing butt surface to obtain a brazed baffle nozzle.

[0073] Preferably, if Figure 2 As shown, two annular channels Ⅰ8 are formed at the pre-assembled connection between the inner shell and the outer shell, with a rectangular cross-section and a length and width of L1 and L2 respectively, for pre-setting brazing material; wherein L1 = 0.8 ~ 0.9 mm, L2 = 0.8 ~ 0.9 mm.

[0074] Preferably, the inner shell after deep processing is plated, specifically: after the outer surface of the inner shell is pickled and degreased, nickel and manganese are plated on the surface to be brazed by chemical electroplating, the nickel layer thickness is 1-2 μm, the manganese layer thickness is 5-10 μm, and the inner surface of the outer shell is pickled and degreased.

[0075] Preferably, the brazing joint surface of the main nozzle structural component is plated, specifically: the surface of the main nozzle structural component to be brazed is pickled and degreased, and then nickel is plated by chemical electroplating, and the thickness of the nickel layer is 5 to 10 μm.

[0076] Preferably, if Figure 3 As shown, the brazing baffle nozzle and the main nozzle structure are pre-assembled, specifically: the brazing baffle nozzle is sleeved on the inner side of the main nozzle structure, and a first annular channel 9, a second annular channel 10, a first brazing surface 11 and a second brazing surface 12 are formed between the outer wall of the brazing baffle nozzle and the inner wall of the main nozzle structure; the first annular channel 9 has a rectangular cross-section, and the length and width are 0.28-0.35 mm and 2.05-2.1 mm respectively, and the second annular channel 10 has a rectangular cross-section, and the width and length are 0.55-0.58 mm and 0.5-0.55 mm respectively; the first annular channel 9 and the second annular channel 10 are used for pre-setting brazing material; the fitting clearance between the first brazing surface 11 and the second brazing surface 12 is 0.02 mm to 0.35 mm.

[0077] Preferably, the annular channel I8 is pre-set with filamentary annular solder Q1, with a specification of φ0.7-0.9mm, 1-2 turns, and fixed by riveting with sample punching points; the first annular channel 9 is pre-set with 1-2 solders Q2 with a size of δ0.2-0.3mm, and the second annular channel 10 is pre-set with 1-2 solders Q2 with a size of δ0.1-0.2mm, and riveting is performed for positioning by sample punching points; the melting point of the solder Q1 is 80-100°C higher than that of the solder Q2. After the brazing assembly formed by the solder Q1 is brazed, it is brazed with the solder ring Q2.

[0078] Preferably, the brazing method is gas shielded brazing and vacuum brazing, wherein the assembly formed by the brazing material Q1 is brazed by gas shielded brazing at a brazing temperature of 940-970°C; the assembly formed by the brazing material Q2 is brazed by vacuum brazing at a brazing temperature of 850-870°C.

[0079] Example

[0080] In the embodiment of the present invention, the baffle nozzle is divided into two parts, the upper part of the baffle nozzle in the low temperature environment and the main nozzle, shell, and inner bottom are integrated by additive manufacturing technology, and the lower part of the baffle nozzle in the high temperature combustion environment adopts a copper alloy brazing structure. Figure 1 As shown, it is mainly composed of a main nozzle structure 1 and a brazing partition nozzle 2 connected by a vacuum brazing method. The main nozzle structure contains 271 main nozzles, 60 upper parts of the brazing partition nozzles, and 60 brazing partition nozzles.

[0081] like Figure 4 As shown, the implementation steps are as follows:

[0082] Step 1: Use computer-aided design software to perform three-dimensional modeling on the main nozzle structure of the injector and optimize the structural model; add a transition chamfer area between the two thin plates and the nozzle, and the angle between the chamfer slope and the injection surface is greater than 45°.

[0083] Step 2: According to the three-dimensional model designed in step 1, the main nozzle structure is formed by laser selective melting forming process, and after forming, stabilization heat treatment, wire cutting substrate, removal of excess powder and support are performed to obtain the main nozzle structure blank;

[0084] Step 3: The main nozzle structure blank obtained in step 2 is subjected to chemical finishing treatment to reduce the surface roughness of the internal tangential hole, and a liquid flow test is performed to verify it. Mechanical processing is performed after the requirements are met.

[0085] Step 4: Wax the main nozzle structural parts blank, machine the brazing surfaces of the upper part of 60 partition nozzles, and process the annular channel 1 with a width × depth of 0.56mmx0.5mm and annular channel 2 with a width × depth of 0.3mmx2.05mm; the brazing surface 1 size on the main nozzle structural parts is 11.21mm, and the brazing surface 2 size is 17.82mm. Dewax treatment is performed after processing.

[0086] Step 5: After degreasing and pickling the surface to be brazed of the product obtained in step 4, nickel plating is performed, and the thickness of the nickel layer is 7 μm.

[0087] Step 6: Install 2xδ0.24mm brazing material Q2 at the first annular channel of the main nozzle structure obtained in step 5, install 2xδ0.12mm brazing material Q2 at the second annular channel, and use sample punching points for riveting positioning.

[0088] Step 7: Process and braze the brazed partition nozzle simultaneously. The outer surface of the inner shell of the brazed partition nozzle is processed with a distance of 1mm, two annular channels with a width of 0.85mm and a depth of 0.9mm. After degreasing the surface to be brazed, nickel and manganese plating are performed. The nickel layer thickness is 1μm and the manganese layer thickness is 8μm. A wire-shaped annular brazing material Q1 with a specification of φ0.8mm is pre-placed in the inner shell annular channel I, with a total of 2 circles. After being fixed by riveting with a sample punch point, it is assembled with the outer shell and formed by gas shielded brazing. The forming temperature is 960℃. After forming, the inlet end is machined to form a brazing butt surface.

[0089] Step 8: After cleaning the surface of the brazing joint surface of the product obtained in step 7, assemble it with the main nozzle structure obtained in step 6. After assembly, braze it in a vacuum brazing furnace to form an injector, and the brazing temperature is 865°C.

[0090] Although the content of the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as a limitation of the present invention. After reading the above content, it will be apparent to those skilled in the art that various modifications and substitutions of the present invention will occur. Therefore, the protection scope of the present invention should be limited by the appended claims.

[0091] The contents not described in detail in the specification of the present invention belong to the common knowledge of the professionals in this field.

Claims

1. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology, characterized in that: include: Carry out 3D modeling of the main nozzle structure of the injector to obtain the main nozzle structure model; Optimizing the main nozzle structure model to obtain the main nozzle model; According to the main nozzle model, laser forming processing is performed to obtain a main nozzle structure blank; Performing chemical finishing treatment on the main nozzle structure blank and conducting a liquid flow test verification; Machining is carried out after the liquid flow test verifies that the requirements are met; The outlet end of the main nozzle structural part blank is machined to obtain the brazing butt surface of the main nozzle structural part; Performing plating treatment on the brazing butt joint surface of the main nozzle structural component; Pre-setting brazing material on the brazing butt joint surface of the main nozzle structural part after the plating treatment to obtain the main nozzle structural part; Processing and brazing the brazed baffle nozzle to obtain the brazed baffle nozzle; The brazing partition nozzle and the main nozzle structural parts are preassembled and placed in a brazing furnace for brazing to obtain a brazing injector.

2. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 1, characterized in that: The brazing injector comprises: a main nozzle structure (1) and a brazing partition nozzle (2), wherein: The main nozzle structure (1) comprises a nozzle and a main structure (5); the main structure (5) is a cylindrical structure, the cylindrical structure comprising a first end head, a middle part and a second end head which are coaxially connected in sequence; the middle part is composed of two thin plates with a hollow interlayer, and the inner thin plate is provided with a through hole; the inner layer of the first end head is provided with a fluid channel; The nozzle is inserted between the two thin plates in the middle part, and the axis of the nozzle is parallel to the axis of the cylindrical structure; one end of the nozzle is flush with the outer surface of the thin plate on one side connected to the first end, and the other end of the nozzle passes through the middle part; The nozzle comprises a plurality of main nozzles (3) and a plurality of baffle nozzle upper parts (4); wherein the baffle nozzle upper parts (4) are coaxially connected to a brazed baffle nozzle (2); the plurality of main nozzles (3) and the plurality of baffle nozzle upper parts (4) are arranged in parallel; the brazed baffle nozzle (2) comprises an inner shell (6) and an outer shell (7); the inner shell (6) is placed inside the outer shell (7) and connected to the surface of the outer shell (7).

3. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 2, characterized in that: The main nozzle structure (1) is made of stainless steel and is formed by additive manufacturing; the brazed partition nozzle (2) is made of copper alloy.

4. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 2, characterized in that: The structural model optimization specifically comprises: adding a transition chamfered area at the connection between the two thin plates in the middle part of the main nozzle structural member (1) and the nozzle, and the angle θ between the chamfered slope and the injection surface is less than 45°.

5. The method for forming a copper-steel brazing coaxial injector based on additive manufacturing process according to claim 1, characterized in that: According to the main nozzle model, laser forming processing is performed to obtain a main nozzle structure blank. The specific method is as follows: According to the main nozzle model, a laser selective melting forming process is adopted to form a main nozzle structure; The formed main nozzle structure is subjected to stabilization heat treatment, the substrate is wire-cut, and excess powder and support are removed to obtain a main nozzle structure blank.

6. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 2, characterized in that: The brazing baffle nozzle is processed and brazed to obtain the brazing baffle nozzle, and the specific method is as follows: Processing and pre-assembling the inner shell and the outer shell to obtain an assembly; Conduct a liquid flow test on the assembly and obtain the test results; According to the test results, the inner shell and the outer shell are further processed until they meet the requirements, thereby obtaining the inner shell and the outer shell after the deep processing; Plating the inner shell after deep processing to obtain a plated inner shell; The plated inner shell is pre-filled with brazing material and connected to the outer shell by brazing to obtain a preliminary sample of a brazed partition nozzle; The inlet end of the brazed baffle nozzle prototype is machined to form a brazing butt surface to obtain a brazed baffle nozzle.

7. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 6, characterized in that: Two annular channels I (8) are formed at the pre-assembly connection between the inner shell and the outer shell, with a rectangular cross section and a length and width of L1 and L2 respectively, for pre-setting brazing material; wherein L1 = 0.8-0.9 mm, L2 = 0.8-0.9 mm.

8. The method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 6, characterized in that: The inner shell body after deep processing is subjected to plating treatment, specifically: after the outer surface of the inner shell body is pickled and degreased, nickel and manganese are plated on the surface to be brazed by chemical electroplating, the nickel layer thickness is 1-2 μm, the manganese layer thickness is 5-10 μm, and the inner surface of the outer shell body is pickled and degreased.

9. The method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 1, characterized in that: The brazing joint surface of the main nozzle structural part is plated, specifically: the surface of the main nozzle structural part to be brazed is pickled and degreased, and then nickel is plated by chemical electroplating, and the thickness of the nickel layer is 5 to 10 μm.

10. The method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 7, characterized in that: The brazing baffle nozzle and the main nozzle structure are preassembled, specifically: the brazing baffle nozzle is sleeved on the inner side of the main nozzle structure, and a first annular channel (9), a second annular channel (10), a first brazing surface (11) and a second brazing surface (12) are formed between the outer wall of the brazing baffle nozzle and the inner wall of the main nozzle structure; the first annular channel (9) has a rectangular cross section, and its length and width are 0.28 to 0.35 mm and 2.05 to 2.1 mm respectively; the second annular channel (10) has a rectangular cross section, and its width and length are 0.55 to 0.58 mm and 0.5 to 0.55 mm respectively; the first annular channel (9) and the second annular channel (10) are used for pre-setting brazing material; and the matching clearance between the first brazing surface (11) and the second brazing surface (12) is 0.02 mm to 0.35 mm.

11. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 10, characterized in that: The annular channel I (8) is pre-set with a filamentary annular solder Q1, with a specification of φ0.7-0.9 mm, 1-2 turns, and fixed by riveting with a sample punch point; the first annular channel (9) is pre-set with 1-2 solders Q2 with a diameter of δ0.2-0.3 mm, and the second annular channel (10) is pre-set with 1-2 solders Q2 with a diameter of δ0.1-0.2 mm, and riveting is performed for positioning by a sample punch point; the melting point of the solder Q1 is 80-100° C. higher than that of the solder Q2, and after the solder assembly formed by the solder Q1 is brazed, it is brazed with the solder ring Q2.

12. A method for forming a copper-steel brazing coaxial injector based on additive manufacturing technology according to claim 11, characterized in that: The brazing methods include gas shielded brazing and vacuum brazing. The assembly formed by the brazing material Q1 is brazed by gas shielded brazing at a brazing temperature of 940-970°C. The assembly formed by the brazing material Q2 is brazed by vacuum brazing at a brazing temperature of 850-870°C.

Citation Information

Patent Citations

  • Manufacturing method of high temperature alloy porous precise injector

    CN104874985A

  • Welding method for multi-part structure of head injector in thrust chamber of liquid-propellant rocket engine

    CN106735829A

  • Combined combustion stabilization device

    CN110805506A

  • Preparation method of injector

    CN113523735A

  • Efficient and stable injector

    CN114215660A