Composite strengthening process for rear oil sealing surface of diesel engine ferrule
By using forging, turning, grinding and rolling processes on the diesel engine ferrule, combined with filling groove finishing and cladding high-strength alloy, the roughness and strength of the contact surface between the ferrule and the rear oil seal are improved, solving the problem of the diesel engine rear The problem of poor sealing performance of oil seals is achieved by achieving higher sealing reliability and wear resistance.
Patent Information
- Application Number
- CN202411028791.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-11
AI Technical Summary
The contact surface between the existing diesel engine ferrule and the rear oil seal has insufficient roughness and strength, resulting in poor sealing performance of the diesel engine rear oil seal and prone to leakage.
A composite strengthening process for the rear oil cover of the diesel engine ferrule is adopted, including forging, turning, milling, drilling, bench cleaning, filling groove finishing and high-strength alloy cladding, grinding, and rolling processing. Distribution design and overall process optimization improve the roughness and strength of the ferrule surface.
It effectively improves the wear resistance and sealing performance of the ferrule sealing surface, solves the problems of poor surface quality of the rear oil cover and low sealing reliability, and extends the service life of the seal.
Smart Images

Figure CN118752185A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diesel engines, and in particular relates to a composite strengthening process for a rear oil cover of a diesel engine ferrule. Background Art
[0002] The crankshaft oil seal is a sealing element used to seal the oil when the engine crankshaft rotates, to prevent the splashing oil in the diesel engine crankcase from leaking out of the diesel engine. It isolates the engine parts that need to be lubricated from the front and rear end parts, and also plays a role in dust prevention. Therefore, whether the oil seal is in good working condition directly affects the reliability of the engine. During operation, the rear oil seal rubber has good elasticity, but there are crushing and cutting edge damage, and the rear oil seal seat is good. After fault analysis, it was confirmed that the roughness and strength of the contact surface between the diesel engine ring and the rear oil seal are important factors affecting the failure of the rear oil seal.
[0003] The outer surface of the diesel engine ring contacts the inner ring of the rubber oil seal to form a dynamic sealing structure, so improving the finish and strength of the outer surface of the ring is the key to improving the sealing effect of the crankshaft oil seal. The original processing technology of the ring is to grind the outer ring after turning, and its roughness can only reach about Ra0.8μm, and the hardness after grinding cannot meet the design requirements.
[0004] The main defects of the existing technical solution are: it cannot meet the high reliability requirements of the high-speed rotating ring dynamic seal, resulting in oil leakage in the rear oil seal of the diesel engine. The main reason is that the roughness value in the original processing solution is low, and the friction and wear of the oil seal-ring moving pair during operation are serious, resulting in premature failure of the rear oil seal and leakage. Secondly, the strength of the outer surface of the ring is not enough, resulting in scratches after being eroded during operation, and the surface quality drops sharply, which leads to seal failure. Summary of the invention
[0005] In view of this, the present invention aims to propose a composite strengthening process for the rear oil cover of a diesel engine ferrule to solve the problem of insufficient strength of the existing rear oil cover of a diesel engine.
[0006] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0007] A diesel engine ferrule rear oil cover composite strengthening process, comprising:
[0008] Forging parts into shapes to obtain blank parts;
[0009] After turning, milling, drilling and cleaning the burrs of the rough parts, the first processed parts are obtained;
[0010] A filling groove is finely machined on the first-machined part corresponding to the installation position of the rear oil seal, and a high-strength alloy is clad on the filling groove to form an alloy layer at the filling groove of the first-machined part;
[0011] The alloy layer at the filling groove of the first processed part is turned to make the outer cylindrical surface of the alloy layer flush with the outer cylindrical surface of the first processed part to obtain the second processed part;
[0012] Grinding the secondary processed parts and the alloy layer at the filling groove thereof to obtain the tertiary processed parts;
[0013] The tertiary processed parts and the alloy layer at the filling groove are rolled to obtain the finished parts.
[0014] Furthermore, the method of fine turning a filling groove corresponding to the rear oil seal installation position on the first processed part, and cladding the filling groove with a high-strength alloy to form an alloy layer at the filling groove of the first processed part includes:
[0015] A filling groove is finely machined on the first processed part corresponding to the installation position of the rear oil seal; wherein the width of the filling groove is greater than the width of the rear oil seal, the depth is at least 1.5 mm, and a transition arc is provided at the bottom edge of the filling groove;
[0016] After preheating the first machined parts after fine turning of the filling groove, a high-strength alloy is clad on the filling groove.
[0017] Furthermore, the diameter R of the transition arc at the bottom edge of the filling groove is 1.5 mm.
[0018] Furthermore, the grinding of the secondary processed part and the alloy layer at the filling groove thereof to obtain the tertiary processed part comprises:
[0019] Grind the secondary processed parts and the alloy layer at the filling groove, control the grinding wheel speed at 20-25m / s, the part speed at 28-32m / min, the feed rate at 0.05-0.2mm / r, the grinding depth at 0.01-0.06mm, and the surface roughness less than Ra0.8μm.
[0020] Furthermore, the three-processed parts and the alloy layer at the filling groove thereof are subjected to rolling processing to obtain the finished parts, including:
[0021] The outer circle center of the alloy layer at the filling groove of the tertiary processed parts is used as the positioning and clamping center. The outer circle center alignment is controlled within 0.01mm, and the tertiary processed parts are measured by table to ensure that the outer circle runout is less than or equal to 0.01mm, so as to realize the clamping of the tertiary processed parts;
[0022] After the tertiary processing parts are clamped, apply low-viscosity oily working fluid on the outer surface of the tertiary processing parts;
[0023] The tertiary processed parts and the alloy layer at the filling groove are rolled multiple times by a diamond rolling cutter to obtain finely processed parts with a surface roughness of less than Ra0.4μm; the rolling speed is controlled at 0.01-0.1mm / r, the feed rate is controlled at 0.005-0.02mm / r, the cutter head radius of the diamond rolling cutter is controlled at 1.0-2.0mm, and the cutter head of the diamond rolling cutter must be free of bumps and scratches.
[0024] Furthermore, the method of using a diamond rolling cutter to perform multiple rolling processes on the tertiary processed parts and the alloy layer at the filling groove thereof to obtain a finely processed part with a surface roughness of less than Ra0.4 μm includes:
[0025] During the first rolling process, the rolling amount should be controlled within 0.01mm;
[0026] During subsequent rolling processes, the rolling amount is controlled at 0.01-0.015 mm each time to obtain a finished part with a surface roughness within Ra0.4 μm.
[0027] Furthermore, the high-strength alloy adopts cobalt-based alloy powder.
[0028] Compared with the prior art, the diesel engine ring rear oil cover composite strengthening process described in the present invention has the following advantages:
[0029] (1) The composite strengthening process for the rear oil cover of a diesel engine ferrule described in the present invention can effectively improve the wear resistance of the ferrule sealing surface by adopting a melt-grind-roll composite process. Good surface performance is obtained by designing the margin distribution between processes and optimizing the overall process. While improving the surface roughness of the ferrule, compressive stress is preset in the near-surface layer of the ferrule, which is beneficial to further improve the working performance of the outer cylindrical surface of the ferrule.
[0030] (2) The composite strengthening process for the rear oil seal of a diesel engine ferrule described in the present invention can effectively improve the sealing performance of the rear oil seal of a diesel engine ferrule, and the processing technology is simple to operate and has high processing efficiency, thus solving the problems of poor surface quality and low sealing reliability of the rear oil seal of a diesel engine in the original method. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:
[0032] Figure 1 It is a schematic diagram of a process for composite strengthening of the rear oil cover of a diesel engine ferrule according to an embodiment of the present invention;
[0033] Figure 2A schematic structural diagram of the cooperation between the ferrule and the rear oil seal in a composite strengthening process for the rear oil seal of a ferrule of a diesel engine according to an embodiment of the present invention;
[0034] Figure 3 It is a schematic structural diagram of a secondary processed part in a composite strengthening process for a rear oil cover of a diesel engine ferrule according to an embodiment of the present invention. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0036] Figure 1 This is a schematic diagram of a composite strengthening process for a diesel engine rear oil seal according to an embodiment of the present invention. This strengthening process can be used to improve the roughness and roughness of the outer surface of the diesel engine rear oil seal to meet product design requirements and improve the reliability of the seal when the diesel engine is working. Figures 1 to 3 As shown, this strengthening process specifically includes the following steps:
[0037] Step 101: Forge the parts to obtain blank parts. Specifically, the parts can be made of steel.
[0038] Step 102, after turning, milling, drilling, and cleaning the burrs of the blank parts, the first processed parts are obtained. The blank parts are processed to obtain the first processed parts whose size specifications meet the processing requirements, so as to facilitate the subsequent further processing of the first processed parts.
[0039] Step 103, fine-machine a filling groove corresponding to the installation position of the rear oil seal on the first processed part, and clad the filling groove with a high-strength alloy to form an alloy layer at the filling groove of the first processed part. Specifically, the high-strength alloy can be made of cobalt-based alloy powder. Cobalt-based alloy is a hard alloy that can withstand various types of wear and corrosion and high-temperature oxidation. That is, it is commonly known as cobalt-chromium-tungsten (molybdenum) alloy. Cobalt-based alloy is a type of alloy that uses cobalt as the main component, contains a considerable amount of nickel, chromium, tungsten and a small amount of alloying elements such as molybdenum, niobium, tantalum, titanium, lanthanum, and occasionally iron. Depending on the composition of the alloy, they can be made into welding wire, and the powder is used for hard surface surfacing, thermal spraying, spray welding and other processes, and can also be made into castings and forgings and powder metallurgy parts. By cladding the high-strength alloy on the filling groove of the first processed part, the strength of the first processed part at the filling groove can be effectively improved, wear can be reduced, and the reliability of the seal at the matching point between the rear oil seal and the ferrule can be improved.
[0040] In actual application, according to the structural characteristics of the ferrule, a filling groove for cladding high-strength alloy is first processed on the outer surface of the ferrule, and then the high-strength alloy is clad to fill the filling groove, which is beneficial to improve the strength of the ferrule at this location.
[0041] Step 104, turning the alloy layer at the filling groove of the first processed part to make the outer cylindrical surface of the alloy layer flush with the outer cylindrical surface of the first processed part, and obtain a second processed part. Specifically, by turning the outer cylindrical surface of the alloy layer to be flush with the outer cylindrical surface of the first processed part, not only can the processing defects of the outer cylindrical surface of the alloy layer be removed, but also it is convenient to process the whole part later, which is conducive to reducing the processing difficulty of the whole part and improving the processing efficiency of the part.
[0042] Step 105: Grind the secondary processed part and the alloy layer at the filling groove to obtain a tertiary processed part. By grinding the part and the alloy layer surface, the surface roughness of the part can be improved and defects such as cracks on the part surface can be eliminated.
[0043] Step 106: Roll the tertiary processed part and the alloy layer at the filling groove to obtain a finished part. By rolling the part and the alloy layer surface, the nominal structural features of the part can be covered, and the purpose of finishing machine strengthening can be achieved, which is conducive to further improving the strength of the part surface, especially the alloy layer.
[0044] The above step 103, precision turning a filling groove corresponding to the rear oil seal installation position on the first processed part, and cladding the filling groove with a high-strength alloy to form an alloy layer at the filling groove of the first processed part, may specifically include the following steps:
[0045] Step 1031, fine-machine a filling groove on the first processed part corresponding to the rear oil seal installation position; wherein the width of the filling groove is greater than the width of the rear oil seal, the depth is at least 1.5 mm, and a transition arc is provided at the bottom edge of the filling groove. By setting the width of the filling groove greater than the width of the rear oil seal, the rear oil seal can be in contact with the alloy layer on the ferrule to form a dynamic sealing structure, thereby utilizing the high strength of the alloy layer to improve the sealing effect and sealing reliability.
[0046] In actual application, the diameter R of the transition arc at the bottom edge of the filling groove can be designed to be 1.5 mm. By setting the transition arc at the bottom edge of the filling groove, it is beneficial to discharge the gas when cladding the high-strength alloy, thereby improving the strength and quality of the alloy layer.
[0047] Step 1032, after preheating the first machined part after fine turning the filling groove, a high-strength alloy is clad on the filling groove.
[0048] Since there is a large temperature difference between the part and the cladding high-strength alloy, preheating the part can effectively reduce the temperature difference, extend the life of the alloy layer, facilitate the discharge of pores in the alloy layer, and reduce the tensile stress caused by cooling shrinkage in the alloy layer and heat-affected zone, thereby inhibiting the generation of cracks in the alloy layer and further improving the quality and strength of the alloy layer. In actual processing, the preheating temperature can be the same or similar to the high-strength alloy cladding temperature to reduce the temperature difference between the two.
[0049] The above step 105, grinding the secondary processed part and the alloy layer at the filling groove thereof to obtain the tertiary processed part, specifically includes the following steps:
[0050] Grind the secondary processed parts and the alloy layer at the filling groove, control the grinding wheel speed at 20-25m / s, control the part speed at 28-32m / min, control the feed rate at 0.05-0.2mm / r, control the grinding depth at 0.01-0.06mm, control the surface roughness to less than Ra0.8μm, and obtain the tertiary processed parts. It should be noted that there should be no cracks on the surface of the tertiary processed parts.
[0051] In actual application, it is necessary to control the grinding speed within a reasonable range to ensure the quality of the parts after grinding. By controlling the grinding wheel speed at 20-25m / s, the part speed at 28-32m / min, the feed rate at 0.05-0.2mm / r, and the grinding depth at 0.01-0.06mm, it can be ensured that there will not be a large amount of grinding heat concentrated on the surface of the part during the alloy layer grinding process, preventing the irreversible physical property changes of the surface metallographic structure of the part, and reducing the possibility of cracking on the surface of the alloy layer due to grinding heat, which is conducive to ensuring the bonding strength between the alloy layer and the part.
[0052] The above step 106, rolling the tertiary processed part and the alloy layer at the filling groove thereof to obtain a finished part, specifically includes the following steps:
[0053] Step 1061, the outer circle center of the alloy layer at the filling groove of the tertiary processing part is used as the positioning and clamping center, the outer circle center alignment is controlled within 0.01mm, and the tertiary processing part is measured by metering to ensure that the outer circle runout is less than or equal to 0.01mm, so as to realize the clamping of the tertiary processing part. By controlling the clamping deviation of the tertiary processing part, it is possible to avoid the cracking of the part or the alloy layer caused by the large deviation between the rolling cutter and the rolling surface during the rolling process, and it is also possible to prevent the rolling cutter head from being damaged.
[0054] Step 1062: After the tertiary processed part is clamped, a low-viscosity oily working fluid is applied to the outer surface of the tertiary processed part. Specifically, the low-viscosity oily working fluid can be an existing cutting fluid. Applying the low-viscosity oily working fluid is beneficial to extending the service life of the rolling cutter head and improving the rolling processing quality of the part surface.
[0055] Step 1063, use a diamond rolling cutter to perform multiple rolling processes on the three-processed parts and the alloy layer at the filling groove thereof, and obtain a finely processed part with a surface roughness of less than Ra0.4μm; wherein the rolling speed is controlled at 0.01-0.1mm / r, the feed rate is controlled at 0.005-0.02mm / r, the cutter head radius of the diamond rolling cutter is controlled at 1.0-2.0mm, and the cutter head of the diamond rolling cutter must be free of bumps and scratches. By controlling the rolling speed, feed rate, and cutter head radius within a relatively small numerical range, it is helpful to prevent damage to the alloy layer during the rolling process.
[0056] Among them, the three-processed parts and the alloy layer at the filling groove are rolled multiple times using a diamond rolling cutter to obtain a finished part with a surface roughness of less than Ra0.4μm, which specifically includes the following steps:
[0057] During the first rolling process, the rolling amount should be controlled within 0.01mm.
[0058] During the subsequent rolling process, the rolling amount is controlled at 0.01-0.015mm each time to obtain a finished part with a surface roughness of less than Ra0.4μm. The fine-tuning function of the diamond rolling cutter can be used to fine-tune the roughness and surface finish after rolling to determine the minimum rolling amount for the pronoun rolling.
[0059] In actual application, after the first rolling process or two rolling processes, the roughness can generally reach within Ra0.4μm. Through multiple rolling processes, the roughness of the part surface can be further ensured and the surface processing quality of the part can be improved. In addition, by using a small rolling amount for the first time and a larger rolling amount for multiple times, it can also effectively prevent damage to the alloy layer, which is conducive to improving the qualified rate of products.
[0060] A composite strengthening process for a rear oil seal surface of a diesel engine ferrule described in an embodiment of the present invention comprises the following steps: forging and pressing parts to obtain blank parts; turning, milling, drilling, and cleaning the burrs on the blank parts to obtain primary processed parts; fine turning a filling groove corresponding to the installation position of the rear oil seal on the primary processed parts, and cladding a high-strength alloy at the filling groove to form an alloy layer at the filling groove of the primary processed parts; turning the alloy layer at the filling groove of the primary processed parts to make the outer cylindrical surface of the alloy layer flush with the outer cylindrical surface of the primary processed parts to obtain secondary processed parts; grinding the secondary processed parts and the alloy layer at the filling groove thereof to obtain tertiary processed parts; rolling the tertiary processed parts and the alloy layer at the filling groove thereof to obtain fine processed parts.
[0061] Compared with the existing technology, the melt-grind-roll composite process can effectively improve the wear resistance of the ring sealing surface. Good surface performance is obtained by designing the allowance distribution between processes and optimizing the overall process. While improving the surface roughness of the ring, compressive stress is preset in the near-surface layer of the ring, which is beneficial to further improve the working performance of the outer cylindrical surface of the ring.
[0062] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A composite strengthening process for the rear oil cover of a diesel engine ferrule. It is characterized in that include: Forging parts into shapes to obtain blank parts; After turning, milling, drilling and cleaning the burrs of the rough parts, the first processed parts are obtained; A filling groove is finely machined on the first-machined part corresponding to the installation position of the rear oil seal, and a high-strength alloy is clad on the filling groove to form an alloy layer at the filling groove of the first-machined part; The alloy layer at the filling groove of the first processed part is turned to make the outer cylindrical surface of the alloy layer flush with the outer cylindrical surface of the first processed part to obtain the second processed part; Grinding the secondary processed parts and the alloy layer at the filling groove thereof to obtain the tertiary processed parts; The tertiary processed parts and the alloy layer at the filling groove are rolled to obtain the finished parts.
2. A diesel engine ring rear oil cover composite strengthening process according to claim 1, It is characterized in that The method of fine turning a filling groove corresponding to the rear oil seal installation position on the first processed part, and cladding the filling groove with a high-strength alloy to form an alloy layer at the filling groove of the first processed part includes: A filling groove is finely machined on the first processed part corresponding to the installation position of the rear oil seal; wherein the width of the filling groove is greater than the width of the rear oil seal, the depth is at least 1.5 mm, and a transition arc is provided at the bottom edge of the filling groove; After preheating the first machined parts after fine turning of the filling groove, a high-strength alloy is clad on the filling groove.
3. A diesel engine ring rear oil cover composite strengthening process according to claim 2, Features: The diameter R of the transition arc at the bottom edge of the filling groove is 1.5 mm.
4. A diesel engine ring rear oil cover composite strengthening process according to claim 1, It is characterized in that The method of grinding the secondary processed part and the alloy layer at the filling groove thereof to obtain the tertiary processed part comprises: Grind the secondary processed parts and the alloy layer at the filling groove, control the grinding wheel speed at 20-25m / s, the part speed at 28-32m / min, the feed rate at 0.05-0.2mm / r, the grinding depth at 0.01-0.06mm, and the surface roughness less than Ra0.8μm.
5. A diesel engine ring rear oil cover composite strengthening process according to claim 1, It is characterized in that The method of rolling the tertiary processed part and the alloy layer at the filling groove thereof to obtain a finished part comprises: The outer circle center of the alloy layer at the filling groove of the tertiary processed parts is used as the positioning and clamping center. The outer circle center alignment is controlled within 0.01mm, and the tertiary processed parts are measured by table to ensure that the outer circle runout is less than or equal to 0.01mm, so as to realize the clamping of the tertiary processed parts; After the tertiary processing parts are clamped, apply low-viscosity oily working fluid on the outer surface of the tertiary processing parts; The tertiary processed parts and the alloy layer at the filling groove are rolled multiple times by a diamond rolling cutter to obtain finely processed parts with a surface roughness of less than Ra0.4μm; the rolling speed is controlled at 0.01-0.1mm / r, the feed rate is controlled at 0.005-0.02mm / r, the cutter head radius of the diamond rolling cutter is controlled at 1.0-2.0mm, and the cutter head of the diamond rolling cutter must be free of bumps and scratches.
6. A diesel engine ring rear oil cover composite strengthening process according to claim 5, It is characterized in that The method of using a diamond rolling cutter to perform multiple rolling processes on the tertiary processed parts and the alloy layer at the filling groove thereof to obtain a finely processed part with a surface roughness of less than Ra0.4 μm includes: During the first rolling process, the rolling amount should be controlled within 0.01mm; During subsequent rolling processes, the rolling amount is controlled at 0.01-0.015 mm each time to obtain a finished part with a surface roughness within Ra0.4 μm.
7. A diesel engine ring rear oil cover composite strengthening process according to claim 1, Features: The high-strength alloy adopts cobalt-based alloy powder.
Citation Information
Patent Citations
method of remanufacturing a seal surface
CN104233285A
Method for intensifying laser cladding layer through ultrasonic rolling
CN107400887A
Repairing technology for ultrasound rolling strengthening of shaft type component surface laser cladding layer
CN109338358A
Machining method for sealing ring groove of sealed bearing
CN113953777A
Piston ring grooves
GB1326480A