Hydrogen conveying pipe and manufacturing method thereof

By using a multi-layer structure of nano-montmorillonite modified phenolic amine hydrogen-blocking curing agent and hydrogen-absorbing epoxy resin in the hydrogen pipeline, combined with a four-step molding method, the problems of hydrogen embrittlement and hydrogen overflow are solved, and efficient hydrogen isolation is achieved. and strength improvement, reducing production costs.

CN118752811APending Publication Date: 2024-10-11OCEAN UNIV OF CHINA

Patent Information

Application Number
CN202410996546.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing metal hydrogen pipelines can easily cause hydrogen embrittlement, causing equipment damage and high maintenance costs. The stiffness of composite materials is low and easy to be damaged, and hydrogen overflow is prone to occur under long-term high pressure conditions.

Method used

It adopts a hydrogen pipe structure composed of an inner lining layer, a connecting layer and a protective layer. The inner lining layer is a glass fiber reinforced composite material made of nano-montmorillonite modified phenolic amine hydrogen blocking curing agent and bisphenol A epoxy resin system. The connecting layer is a hydrogen-absorbing epoxy resin composed of polyethylene glycol-modified phenolic amine hydrogen-absorbing curing agent and bisphenol A epoxy resin. It is prepared through a four-step molding method, including winding molding of the inner lining layer, infusion of the connecting layer, and spinning. Pressed and cut to form.

Benefits of technology

Effectively reduce hydrogen leakage, improve structural strength and mechanical properties, reduce production costs, avoid hydrogen embrittlement and hydrogen overflow, and improve the integrity and production efficiency of hydrogen pipelines.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118752811A_ABST
    Figure CN118752811A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of hydrogen conveying pipes, and particularly relates to a hydrogen conveying pipe and a manufacturing method thereof. The novel hydrogen conveying pipe structure is composed of an impact-resistant and anti-aging metal protection outer layer, a glass fiber composite material inner weighing layer for preventing hydrogen from overflowing, reducing the weight of the structure and improving the strength of the structure, and a connecting layer for absorbing escape hydrogen, preventing metal hydrogen embrittlement and connecting the inner layer and the outer layer. The novel hydrogen conveying pipe adopts a four-step manufacturing and forming method, the method is a novel manufacturing method integrating composite pipe integral forming, metal layer surface strengthening and resin matrix in-situ curing, and meanwhile, a novel auxiliary manufacturing tool matched with the manufacturing method is designed. According to the novel hydrogen conveying pipe structure and the manufacturing method thereof, the hydrogen conveying pipe can have the excellent characteristics of hydrogen overflow prevention, light weight, high strength, high production efficiency, economy and the like, and the structure and the manufacturing design of the novel hydrogen conveying pipe structure can also be used for transportation of oil extraction pipes and other media while the requirement of hydrogen conveying operation is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of hydrogen transmission pipes, and in particular relates to a hydrogen transmission pipe and a manufacturing method thereof. Background Art

[0002] Hydrogen has the lowest density of all gases, so it can enter the crystal lattices of many metals, causing "hydrogen embrittlement" and causing rupture or damage to metal pipes, resulting in production interruptions, safety accidents, etc., and then causing large economic losses due to equipment maintenance, replacement, and production stagnation. Existing metal hydrogen pipes usually use internal coatings to prevent hydrogen from contacting the metal pipes, but the coating is easy to fall off, resulting in high subsequent maintenance costs. Therefore, there are disadvantages in using a single metal pipe structure as a hydrogen pipe.

[0003] In view of this, the prior art discloses that composite materials have good performance in hydrogen resistance, but their rigidity is low and they are prone to damage after long-term use, which increases the overall cost of hydrogen pipeline construction and maintenance. Therefore, there are also disadvantages in using a single composite material as a hydrogen pipeline. In addition, the structural design and manufacturing method of the pipeline still have the problem of hydrogen overflow, and the existing hydrogen pipeline is still prone to hydrogen embrittlement when it is under high pressure for a long time. Summary of the invention

[0004] Based on the above purpose, the first technical solution of the present application provides a hydrogen transmission pipe, including an inner lining layer, a connecting layer, and a protective layer; wherein the inner lining layer is made of a hydrogen-blocking glass fiber reinforced composite material, the connecting layer is made of a hydrogen-absorbing epoxy resin, and the protective layer is a steel pipe.

[0005] Furthermore, the hydrogen-blocking glass fiber reinforced composite material is a glass fiber reinforced composite material of a nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and a bisphenol A epoxy resin system.

[0006] Furthermore, the hydrogen absorbing epoxy resin is composed of a polyethylene glycol-modified phenolic amine hydrogen absorbing curing agent and a bisphenol A epoxy resin.

[0007] Furthermore, the thickness of the lining layer is 0.1-5 mm, the thickness of the connecting layer is 0.1-5 mm, the thickness of the protective layer is 1-15 mm, and the diameter of the protective layer steel pipe is 50-500 mm.

[0008] The second technical solution of the present invention provides a method for preparing the above-mentioned hydrogen transmission pipe, wherein the hydrogen transmission pipe is prepared by a four-step molding method using a molding fixture; the molding fixture comprises a buckle (1), a buckle (2), a resin transfer molding (RTM) channel (3) located on the buckle (2), a fixture disc (4) and a disc groove (5);

[0009] The buckle (1) and the buckle (2) are detachable, and there is a height difference between the buckle (1) and the buckle (2), and the height difference is 0.1-10 mm; the length of the buckle (1) is 100-300 mm, and the length of the buckle (2) is 50-100 mm.

[0010] Furthermore, the four-step molding method comprises:

[0011] S1. Inner lining molding: Connect the buckle (2) to the core mold to wrap the inner lining, and then insert the protective layer steel pipe into the fixture;

[0012] S2. Connection layer injection: connect the buckle (1) with the disc groove (4), the buckle (2) is close to the inner layer of the protective layer steel pipe to provide support, the buckle (1) is close to the outer layer of the protective layer steel pipe and cooperates with the buckle (2) to fix the protective layer steel pipe; inject epoxy resin through the reserved RTM channel of the buckle (2).

[0013] S3. Trinity spinning: Through the rotation of the spinner and the extrusion of the spinning wheel, the steel pipe is reduced in diameter, the pipe is integrally spun, the metal surface is finely grained and strengthened, and the hydrogen absorbing / blocking resin is in-situ cured by the self-heat of spinning;

[0014] S4. Cutting and forming: cutting the unformed part along the chuck to obtain the hydrogen delivery pipe.

[0015] Furthermore, the inner lining layer is formed by wet winding of fibers, specifically, the nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and the glass fiber reinforced composite material of the bisphenol A epoxy resin system are wet-wound and then inserted into the outer steel pipe to form a 1-20mm fitting gap.

[0016] Furthermore, the molding thickness is 1-5 mm, the inner layer diameter is 50-500 mm, the steel pipe is Q345 steel, the diameter is 50-500 mm, and the difference between the inner and outer layer diameters is 0.1-10 mm.

[0017] Furthermore, the hydrogen absorbing epoxy resin in S2 is injected by RTM technology to connect the outer steel tube and the inner glass fiber tube, and the S3 is spun with a core mold speed of 60r / min to 3000r / min, a downward pressure of 1-20mm, and a spinning heat generation temperature of 50-400°C.

[0018] And, a hydrogen transmission pipe prepared according to the above preparation method.

[0019] The beneficial effects of this application are:

[0020] The present invention comprises an inner lining layer, a connecting layer and a protective layer which are sequentially arranged from the inside to the outside. The inner lining layer is a glass fiber reinforced composite material of a nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and a bisphenol A epoxy resin system, and the connecting layer is a hydrogen-absorbing epoxy resin composed of a polyethylene glycol-modified phenolic amine hydrogen-absorbing curing agent and a bisphenol A epoxy resin. The double-layer structure coupling effect of the inner lining layer and the connecting layer can effectively reduce hydrogen leakage; and the inner lining layer has a certain supporting strength and the coupling effect with the protective layer steel pipe jacket provides double-layer supporting protection.

[0021] The four-step molding method uses corresponding molding methods for different layer structures. The fiber wet winding molding of the hydrogen barrier lining layer can achieve a higher structural strength of the lining layer and accurately control the dosage; the RTM (resin transfer molding channel) technology of the epoxy resin of the connecting layer can reduce the generation of bubbles, enhance the mechanical properties and durability of the glue layer and improve the consistency of the product; the spin forming of the steel pipe protective layer can integrate surface strengthening, pipe molding and epoxy resin curing into one. The three are carried out simultaneously, which can improve the integrity of the hydrogen transmission pipe, improve production efficiency and reduce production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Attached Figure 1 It is a schematic diagram of the structure of the hydrogen transmission pipe of the present invention;

[0023] Attached Figure 2 It is a general diagram of the fixture in the molding process of the present invention;

[0024] Attached Figure 3 It is a composition diagram of the clamp of the present invention;

[0025] Attached Figure 4 is a flow chart of the present invention;

[0026] Attached Figure 5 This is the result of the hydrogen leakage test of the L360QS type coated hydrogen transmission pipe;

[0027] Attached Figure 6 This is a diagram showing the results of a hydrogen leakage experiment on the hydrogen transmission pipe of the present application. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific embodiments. This implementation case is implemented based on the technology of the present invention, and a detailed implementation method and specific operation process are now given to illustrate that the present invention is creative, but the protection scope of the present invention is not limited to the following embodiments.

[0029] Example 1 A hydrogen transport pipe

[0030] like Figure 1As shown, this embodiment discloses a hydrogen transmission pipe, which is composed of an inner lining layer, a connecting layer, and a protective layer from the inside to the outside; wherein the inner lining layer is made of a hydrogen-blocking glass fiber reinforced composite material, preferably a glass fiber reinforced composite material of a nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and a bisphenol A epoxy resin system, the connecting layer is made of a hydrogen-absorbing epoxy resin, preferably a polyethylene glycol-modified phenolic amine hydrogen-absorbing curing agent and a bisphenol A epoxy resin, and the protective layer is a steel pipe. wherein the thickness of the inner lining layer is 0.1-5mm, the thickness of the connecting layer is 0.1-5mm, the thickness of the protective layer is 1-15mm, and the diameter of the protective layer steel pipe is 50-500mm.

[0031] In this embodiment, the preparation of the glass fiber reinforced composite material of the nano-montmorillonite modified phenolic amine hydrogen-blocking curing agent and bisphenol A epoxy resin system is as follows:

[0032] S1. The material preparation is divided into four groups: Component A uses E-51 and E-44 bisphenol A epoxy resin as the resin matrix; Component B uses cardanol-based phenolic amine curing agent; Component C uses nano-montmorillonite; Component D is glass fiber. The phenolic substance is cardanol; the amine substance is meta-phenylenediamine; and the aldehyde substance is polyformaldehyde. The mass ratio of component A, component B, component C and component D is 10:4:4:9.

[0033] S2. Mix and stir components A, B and C at 40-60°C for 5-20 minutes, add a catalyst, raise the temperature to 80-100°C, and keep the temperature for reaction for 0.5-2 hours.

[0034] S2. After the three components A, B and C are mixed according to the mass ratio, glass fiber is added according to the mass ratio to ensure that they are fully wetted.

[0035] S3. Curing at room temperature for 6 hours, and obtaining the product by fiber wet winding molding.

[0036] The cross-linking and curing between the components form a colloidal material with a certain mechanical strength, which has the advantages of heat resistance, corrosion resistance, good mechanical properties, strong adhesion, etc. Introducing cardanol as a phenolic substance into the curing agent system through the Mannich reaction can greatly improve the colloidal mechanical properties and sealing of the epoxy structural adhesive. At the same time, montmorillonite has a large specific surface area and interlayer spacing, which can effectively hinder the penetration and diffusion of hydrogen molecules, thereby improving the hydrogen barrier properties of epoxy resin. The nanosheet structure of montmorillonite can enhance the mechanical properties of epoxy resin, improve its strength and toughness, and help to extend the service life of the material. The addition of glass fiber further enhances its mechanical properties and provides good support.

[0037] In this embodiment, the polyethylene glycol-modified phenolic amine hydrogen absorption curing agent and bisphenol A epoxy resin are prepared as follows:

[0038] S1. Component A uses E-44 and E-51 bisphenol A epoxy resin; component B uses cardanol-based phenolic amine curing agent; component C uses polyethylene glycol. The phenolic substance is cardanol; the amine substance is meta-phenylenediamine; and the aldehyde substance is paraformaldehyde. The mass ratio of component A, component B and component C is 10:4:4.

[0039] S2. Mix and stir the phenol solution at 40-60°C for 5-20 minutes, add the catalyst, and when the catalyst is completely dissolved, raise the temperature to 80-100°C, and keep the temperature for 0.5-2 hours. After the reaction is completed, cool the reaction system to 70-90°C, add amines, mix well, add aldehydes in batches, and when the aldehydes are dissolved, raise the temperature to 80-100°C, keep the temperature for 1-4 hours, and add polyethylene glycol according to the mass ratio.

[0040] S3. Raise the temperature to 90-110°C and connect a vacuum decompression device at the same time, and perform a dehydration reaction under vacuum conditions for 2-4 hours to obtain a connecting layer hydrogen-absorbing epoxy resin composed of a polyethylene glycol-modified phenolic amine hydrogen-absorbing curing agent and a bisphenol A epoxy resin.

[0041] By introducing polyethylene glycol segments, the barrier capacity of epoxy resin to hydrogen can be increased, reducing the penetration and leakage of hydrogen. Polyethylene glycol usually has good flexibility, and the modified epoxy resin is more tough and impact-resistant.

[0042] The coupling effect of the double-layer structure of the lining layer and the connecting layer can effectively reduce hydrogen leakage; and the lining layer has a certain supporting strength and the coupling effect with the protective layer steel pipe jacket provides double-layer supporting protection.

[0043] Example 2 Preparation method of hydrogen transport pipe

[0044] In the prior art, the structural design and manufacturing method of the pipeline still have the problem of hydrogen overflow, and the existing hydrogen transmission pipeline is still prone to hydrogen embrittlement when it is under high pressure for a long time.

[0045] To this end, the present application provides a method for preparing a hydrogen transmission pipe by a four-step molding method, and the four-step molding method is completed on the same equipment (a large three-wheel high-power spinning equipment). For the fiber wet winding molding of the hydrogen barrier lining layer, a higher structural strength of the lining layer can be achieved and the dosage can be precisely controlled; for the vacuum infusion technology or injection molding technology of the epoxy resin of the connecting layer, the generation of bubbles can be reduced, the mechanical properties and durability of the glue layer can be enhanced, and the consistency of the product can be improved; for the spinning molding of the steel pipe protective layer, surface strengthening, pipe molding and epoxy resin curing can be integrated into one, and the three are carried out simultaneously, which can improve the integrity of the hydrogen transmission pipe, improve production efficiency, and reduce production costs.

[0046] In order to achieve the above requirements, the present application first discloses a clamp for forming, such as Figure 2 , Figure 3 As shown, it includes the following structure:

[0047] The molding fixture comprises a buckle (1), a buckle (2), a resin transfer molding (RTM) channel (3) located on the buckle (2), a disc groove (4) and a fixture disc (5);

[0048] The buckle (1) and the buckle (2) are detachable, and there is a height difference between the buckle (1) and the buckle (2), and the height difference is 0.1-10 mm; the length of the buckle (1) is 100-300 mm, and the length of the buckle (2) is 50-100 mm.

[0049] The buckle (1) is a buckle for supporting the protective layer, and the buckle (1) is fixed to ensure the stability of the protective layer of the hydrogen pipe during the process of spinning and compressing the diameter; the buckle (2) is a buckle for supporting the inner lining layer, and the buckle (2) is fixed to ensure the stability of the inner lining layer of the hydrogen pipe during the winding and molding process. At the same time, the buckle (2) can provide support for the inner wall of the protective layer and achieve double-effect clamping with the buckle (1); the height difference between the buckle (1) and the buckle (2) is the thickness of the protective layer to achieve the effect of layered fixing.

[0050] The resin transfer molding (RTM) channel (3) is a vacuum infusion channel. By reserving the RTM channel, the output pipe of the RTM equipment can be connected to the fixture to achieve the infusion of the connection layer resin.

[0051] The clamp disc provides a fixed position for the buckle (1) and the buckle (2), and the groove fixes the buckle (1) and the buckle (2).

[0052] In addition, in a specific embodiment, the buckle component is divided into a main body and an external buckle, which can flexibly support the multi-layer structure, and can provide support while supporting, realize double-effect fixation, and can effectively maintain the integrity of each layer structure. Figure 3 shown.

[0053] The diameter and thickness of the fixture disc (5) are: diameter: 40-500mm, thickness: 10-50mm.

[0054] In a further embodiment, Figure 4 As shown, the four-step molding method includes:

[0055] S1. Inner lining molding: Connect the buckle (1) to the core mold (the mold for wet winding of the inner lining fiber), such as Figure 4 (1), the inner lining layer is wound into shape, as shown in Figure 4 (2), then the outer steel pipe is put into the fixture, as shown in Figure 4 (3) as shown;

[0056] S2. Connection layer pouring: Connect the buckle (1) with the groove of the disc, such as Figure 4 As shown in (3)-(a), the buckle (2) is tightly attached to the inner layer of the protective layer steel pipe to provide support, such as Figure 4 As shown in (3)-(b), the buckle (1) is closely attached to the outer layer of the steel pipe and cooperates with the buckle (2) to fix the outer steel pipe; the RTM channel is reserved through the buckle (2), such as Figure 4 (4)-(c) as shown, epoxy resin is poured, such as Figure 4 (5) as shown.

[0057] S3. Three-in-one spinning: The steel tube is reduced in diameter by spinning machine operation to achieve resin solidification, such as Figure 4 As shown in (6)(7);

[0058] S4. Cutting and forming: Cut the unformed part along the chuck to obtain the hydrogen delivery pipe. Figure 4 As shown in (8)(9).

[0059] Furthermore, the inner lining layer is formed by wet fiber winding, specifically, the nano-montmorillonite modified phenolic amine system hydrogen-blocking epoxy resin-based glass fiber reinforced composite material is drawn and wound into shape, and then the outer steel pipe is used to insert the composite material.

[0060] Furthermore, the molding thickness is 2 mm, the inner layer diameter is 14.7 cm, and the steel pipe is Q345 steel with a diameter of 15.1 cm.

[0061] Furthermore, the epoxy resin in S2 is injected by vacuum infusion technology or injection molding technology.

[0062] In the S3, when the epoxy resin of the lining layer and the connecting layer are synchronously cured by spinning heat, the spinning speed is controlled so that the spinning heat temperature reaches 50-300° C. to achieve the curing of the epoxy resin. The spinning machine used for spinning is a double-wheel spinning machine or a three-wheel spinning machine.

[0063] The three-in-one molding adopts the method of spinning and compressing the diameter to simultaneously achieve the surface strengthening of the steel pipe of the protective layer of the hydrogen transmission pipe; to achieve a close combination of the three-layer structure of the lining layer, the connecting layer and the protective layer; the heat generated during the spinning process is used to achieve the synchronous curing of the epoxy resin of the lining layer and the connecting layer by spinning heat; the four-step molding method uses corresponding molding methods for different layer structures, and the fiber wet winding molding of the hydrogen barrier lining layer can achieve a higher structural strength of the lining layer and accurately control the dosage; the RTM (resin transfer molding channel) technology of the epoxy resin of the connecting layer can reduce the generation of bubbles, enhance the mechanical properties and durability of the glue layer, and improve the consistency of the product; for the spinning molding of the steel pipe protective layer, the surface strengthening, pipe molding and epoxy resin curing can be integrated into one, and the three are carried out simultaneously, which can improve the integrity of the hydrogen transmission pipe, improve production efficiency, and reduce production costs.

[0064] Test Example 1 Hydrogen Leakage Test

[0065] Experimental method: The double electrolytic cell method was used to study the effect of hydrogen permeation on the coating stripping of pipeline steel surface. The coated side was used as the detection surface, and the other side (without coating) was used as the hydrogen charging surface. The detection solution was injected into the container of the detection surface. The sample was used as the working electrode, the saturated calomel electrode was used as the reference electrode, and the platinum electrode was used as the auxiliary electrode. The open circuit potential of the detection surface was monitored by the Coster CS350 electrochemical workstation. After the open circuit potential was stable, the hydrogen charging liquid was injected into the cathode cell. The cathode hydrogen charging current density was 0, 5, 10, and 20 mA / cm 2 The surface morphology and cross-sectional morphology of the samples before and after coating peeling were observed by scanning electron microscopy (SEM).

[0066] The hydrogen transmission pipe prepared in Example 2 of the present application and the commonly used coated hydrogen transmission pipe (L360QS) on the market were subjected to hydrogen leakage test. The test results are as follows: Figure 5 , Figure 6 As shown: Figure 5 Figures a, b, c, and d show the microscopic morphology of the coated steel section of the L360QS pipeline after hydrogen filling under different conditions. Figure 6 This is the microscopic morphology of the cross section of the hydrogen transmission tube prepared in Example 2 after hydrogen filling.

[0067] like Figure 5 As shown in the figure, under the condition of no hydrogen penetration, the protective performance of the coating decreases with the extension of immersion time, but the coating surface will not peel off ( Figure 5 a); During electrochemical hydrogen charging, due to the concentration gradient of hydrogen atoms, hydrogen atoms will penetrate the sample and gather at the coating / metal interface; when the pressure generated by the accumulated hydrogen atoms is greater than the adhesion of the coating, the coating will bubble locally ( Figure 5 bd).

[0068] and Figure 6 Even at a hydrogen charging current density of 20 mA / cm 2 There was no bubbling phenomenon, which shows that compared with the coated hydrogen transmission pipe, the present application effectively prevents coating peeling and bubbling after the inner lining hydrogen barrier layer and the hydrogen absorption connecting layer are coupled by the three-in-one molding method, and can prevent hydrogen overflow and absorb escaped hydrogen.

[0069] Test Example 2 Mechanical Properties Test

[0070] 2. Experimental method: The commonly used hydrogen pipeline steel, ASME B31.12-2014 (the "Hydrogen Pipeline and Pipeline" standard issued by the American Society of Mechanical Engineers) defines several types of steel that can be used for hydrogen pipelines in API SPEC 5L. The pipeline steel materials that can be used for hydrogen pipelines specified in the standard are compared with the hydrogen pipeline prepared in Example 2 of this application for mechanical property testing. First, prepare tubular specimens of the same size and shape as the sample; install the prepared sample into the fixture of the testing machine to ensure that the sample is clamped; start the testing machine, apply tension to the sample at a constant rate and record the deformation of the sample and the applied force until the sample begins to produce plastic deformation as the yield point; determine the yield strength of the sample based on the recorded data.

[0071] Experimental results: As shown in Table 1: The results of mechanical testing of the novel hydrogen transmission pipe in the present invention show that the hydrogen transmission pipe of the present application has stronger yield strength and tensile strength, thereby ensuring the stable operation of the hydrogen transmission pipe. And its transmission pressure can reach 10MPa, which is higher than 4-5Mpa in the daily hydrogen transmission line, and can transport hydrogen more efficiently.

[0072] Table 1 Mechanical properties test results

[0073] Material Type(API5L) X42 X52 X56 X60 X65 X70 X80 Example 2 Yield strength / MPa 289.6 358.5 386.1 413.7 448.2 482.7 551.6 597.6 Tensile strength / MPa 413.7 455.1 489.5 517.1 530.9 565.4 620.6 679.3 Maximum allowable pressure / MPa 20.68 20.68 20.68 20.68 20.68 10.34 10.34 10.34

[0074] Finally, it should be noted that the above implementation cases are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred implementation cases, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.

Claims

1. A hydrogen transmission pipe, characterized in that: It includes an inner lining layer, a connecting layer and a protective layer; wherein the inner lining layer is made of a hydrogen-blocking glass fiber reinforced composite material, the connecting layer is made of a hydrogen-absorbing epoxy resin, and the protective layer is a steel pipe.

2. The hydrogen transport pipe according to claim 1, characterized in that: The hydrogen-blocking glass fiber reinforced composite material is a glass fiber reinforced composite material of a nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and a bisphenol A epoxy resin system.

3. The hydrogen transport pipe according to claim 1, characterized in that: The hydrogen absorbing epoxy resin is composed of a polyethylene glycol-modified phenolic amine hydrogen absorbing curing agent and a bisphenol A epoxy resin.

4. The hydrogen transport pipe according to claim 1, characterized in that: The thickness of the lining layer is 0.1-5mm, the thickness of the connecting layer is 0.1-5mm, the thickness of the protective layer is 1-15mm, and the diameter of the protective layer steel pipe is 50-500mm.

5. The method for preparing the hydrogen transmission pipe according to any one of claims 1 to 4, characterized in that: The hydrogen transport pipe is manufactured by a four-step molding method using a molding fixture; the molding fixture comprises a buckle (1), a buckle (2), a resin transfer molding (RTM) channel (3) located on the buckle (2), a fixture disc (4) and a disc groove (5); The buckle (1) and the buckle (2) are detachable, and there is a height difference between the buckle (1) and the buckle (2), and the height difference is 0.1-10 mm; the length of the buckle (1) is 100-300 mm, and the length of the buckle (2) is 50-100 mm.

6. The preparation method according to claim 5, characterized in that: The four-step molding method comprises: S1. Inner lining molding: Connect the buckle (2) to the core mold to wrap the inner lining, and then insert the protective layer steel pipe into the fixture; S2. Connection layer injection: connect the buckle (1) with the disc groove (4), the buckle (2) is close to the inner layer of the protective layer steel pipe to provide support, the buckle (1) is close to the outer layer of the protective layer steel pipe and cooperates with the buckle (2) to fix the protective layer steel pipe; inject epoxy resin through the reserved RTM channel of the buckle (2). S3. Trinity spinning: Through the rotation of the spinner and the extrusion of the spinning wheel, the steel pipe is reduced in diameter, the pipe is integrally spun, the metal surface is finely grained and strengthened, and the hydrogen absorbing / blocking resin is in-situ cured by the self-heat of spinning; S4. Cutting and forming: cutting the unformed part along the chuck to obtain the hydrogen delivery pipe.

7. The preparation method according to claim 6, characterized in that: The inner lining layer is formed by wet winding of fibers, specifically, the nano-montmorillonite-modified phenolic amine hydrogen-blocking curing agent and the glass fiber-reinforced composite material of the bisphenol A epoxy resin system are wet-wound and then inserted into the outer steel pipe to form a 1-20 mm matching gap.

8. The preparation method according to claim 7, characterized in that: The molding thickness is 1-5mm, the inner layer diameter is 50-500mm, the steel pipe is Q345 steel, the diameter is 50-500mm, and the difference between the inner and outer layer diameters is 0.1-10mm.

9. The preparation method according to claim 6, characterized in that: In the S2, the hydrogen-absorbing epoxy resin is injected through RTM technology to connect the outer steel pipe and the inner glass fiber pipe. In the S3, the spinning is performed with a core mold of 60r / min to 3000r / min, a downward pressure of 1-20mm, and a spinning heat generation temperature of 50-400°C.

10. A hydrogen transmission pipe prepared according to any one of the preparation methods according to claims 6-9.

Citation Information

Patent Citations

  • Composite pipeline for hydrogen conveying and hydrogen leakage monitoring method

    CN114413186A

  • Nonmetal composite pipe for conveying hydrogen and manufacturing method

    CN115773407A

  • Lining regeneration intelligent hydrogen conveying pipeline

    CN116379227A

  • High-vacuum multi-layer heat insulation hose with vacuum male plug for liquid hydrogen transmission

    CN218883390U

  • Method for manufacturing compositely molded 99-mpa-grade hydrogen storage container for hydrogen refueling station

    WO2024041262A1

Cited By

  • Forming device for forming hydrogen-resistant material layer on inner wall of hydrogen-resistant steel cylinder

    CN122500882A