In-situ tin-doped carbon material and preparation method and application thereof

Through the preparation method of in-situ tin-doped carbon materials, the problem of insufficient energy density of lithium-ion battery negative electrode materials is solved, high specific capacity and stability are achieved, and a low-cost, simple-process solution is provided, which is suitable for lithium-ion batteries. Battery negative electrode material.

CN118754091APending Publication Date: 2024-10-11SHIHEZI UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410758454.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The energy density of existing negative electrode materials for lithium-ion batteries is insufficient to meet the growing requirements of energy storage systems, and the modification methods of commercial graphite have problems such as high cost and complex processes.

Method used

Using the preparation method of in-situ tin-doped carbon materials, by reacting cotton straw powder with anhydrous tin tetrachloride in a cyclohexane solvent, after drying, grinding and calcining, tin with high specific capacity and stability was prepared Doped carbon materials.

Benefits of technology

The preparation of tin-doped carbon materials with low cost, simple process and low energy consumption has been achieved, which has significantly improved the first discharge specific capacity and stability of lithium-ion battery anode materials, and has great application potential.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754091A_ABST
    Figure CN118754091A_ABST
Patent Text Reader

Abstract

The invention relates to an in-situ tin-doped carbon material and a preparation method and application thereof. The invention relates to a preparation method of an in-situ tin-doped carbon material, which comprises the following steps: adding cotton straw powder into an organic solvent, uniformly stirring and mixing, adding anhydrous tin tetrachloride, and drying and calcining after the reaction is finished. According to the in-situ tin-doped carbon material and the preparation method and application thereof, the preparation method has the advantages of being simple in process, low in cost and low in energy consumption, and the tin-carbon composite material with high first discharge specific capacity and excellent stability is prepared, so that the in-situ tin-doped carbon material has great application potential in lithium ion battery negative electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and in particular relates to an in-situ tin-doped carbon material and a preparation method and application thereof. Background Art

[0002] In the past few decades, the energy demand has increased rapidly due to the growing demand for portable electronic devices, which have been widely used. Compared with other secondary metal-ion batteries, lithium-ion batteries have higher energy density, longer life and lighter design, however, the energy density of lithium-ion batteries still needs to be improved because the current commercial graphite is not enough to meet the growing requirements for energy storage systems. Therefore, it is necessary to develop new anode materials with higher specific capacity and stable performance to meet the industrialization requirements at the commercial level.

[0003] Depending on the negative electrode material, it can be divided into carbon-based materials, metal oxides and conductive polymers. Among them, carbon-based materials are the most promising negative electrode materials. They are abundant and inexpensive, but their capacity, conductivity and structural stability still cannot meet future applications, so they need to be modified according to different structures. At present, the most common methods for modifying carbon-based materials include structural regulation, heteroatom doping and composite material design. Heteroatom (nitrogen, sulfur, phosphorus, etc.) doping carbon-based materials can optimize the local electronic structure of carbon-based materials, thereby improving their conductivity. Doping with nitrogen, sulfur, phosphorus and other elements has been shown to help improve the electrochemical properties of carbon materials. Metallic tin is non-toxic and inexpensive, with a high theoretical specific capacity (994mAh·g -1 ), is considered as one of the optional materials for the negative electrode of lithium-ion batteries.

[0004] Based on this, the present invention proposes an in-situ tin-doped carbon material and a preparation method and application thereof, which provides a new idea for designing heteroatom-doped carbon materials for lithium battery negative electrodes. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing an in-situ tin-doped carbon material, which has simple process, low cost and low energy consumption.

[0006] In order to achieve the above purpose, the technical solution adopted is:

[0007] A method for preparing an in-situ tin-doped carbon material comprises: adding cotton straw powder into an organic solvent, stirring and mixing evenly, adding anhydrous tin tetrachloride, and drying, grinding and calcining after the reaction is completed.

[0008] Furthermore, the organic solvent is cyclohexane.

[0009] Furthermore, the mass volume ratio of the cotton straw powder to anhydrous tin tetrachloride is 1g:15-20ml.

[0010] Furthermore, the drying is vacuum drying at a temperature of 75-85° C. for 10-14 hours.

[0011] Furthermore, the drying temperature is 80° C. and the drying time is 12 hours.

[0012] Furthermore, the calcination temperature is 600-800° C. and the calcination time is 1.5-2.5 h.

[0013] Furthermore, the calcination temperature is 700° C. and the calcination time is 2 h.

[0014] Another object of the present invention is to provide an in-situ tin-doped carbon material, which is prepared by the above-mentioned preparation method and has the advantages of high first discharge specific capacity and excellent stability.

[0015] Another object of the present invention is to provide application of the above-mentioned in-situ tin-doped carbon material in negative electrode materials of lithium-ion batteries.

[0016] Compared with the prior art, the present invention has the following beneficial effects:

[0017] 1. The technical solution of the present invention uses biomass waste cotton straw and anhydrous tin tetrachloride as raw materials, and has the advantage of low cost.

[0018] 2. The technical solution of the present invention prepares tin atom-doped cotton straw carbon material by in-situ doping. The preparation method has the advantages of simple process, low cost and low energy consumption, and solves the problems of complex process and long preparation cycle.

[0019] 3. The technical solution of the present invention prepares a tin-carbon composite material with high first discharge specific capacity and excellent stability, which exhibits excellent specific capacity and stability in lithium-ion battery tests, and thus has great application potential in lithium-ion battery negative electrode materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The Sn-CS-Carbon-4 tested in Example 1 of the present invention is 50mAg -1 Charge and discharge curves under current density.

[0021] Figure 2 The carbon material CS-Carbon prepared in Comparative Example 1 of the present invention is -1 Charge and discharge curves under current density.

[0022] Figure 3 The Sn-CS-Carbon-3 tested in Example 2 of the present invention is 50mAg -1 Charge and discharge curves under current density.

[0023] Figure 4 The Sn-CS-Carbon-5 tested in Example 3 of the present invention is 50mAg -1 Charge and discharge curves under current density. DETAILED DESCRIPTION

[0024] In order to further illustrate the in-situ tin-doped carbon material and its preparation method and application of the present invention and achieve the intended purpose of the invention, the following is a detailed description of the in-situ tin-doped carbon material and its preparation method and application, its specific implementation method, structure, characteristics and efficacy proposed in accordance with the present invention in combination with the preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures or characteristics in one or more embodiments may be combined in any suitable form.

[0025] The following will further introduce in detail an in-situ tin-doped carbon material and its preparation method and application in conjunction with specific embodiments of the present invention:

[0026] The present invention provides a method of preparing a tin atom-doped biomass-derived porous carbon material by in-situ doping using biomass waste cotton straw and anhydrous tin tetrachloride as raw materials, and applying the material to the negative electrode of a lithium-ion battery. The in-situ tin atom doping method provided by the present invention provides a new theoretical idea for designing a new tin atom-doped carbon material for a negative electrode material of a lithium-ion battery, and is a low-cost, simple process, and green and environmentally friendly process. The technical solution of the present invention is:

[0027] A method for preparing an in-situ tin-doped carbon material comprises: adding cotton straw powder into an organic solvent, stirring and mixing evenly, adding anhydrous tin tetrachloride to react, and drying, grinding and calcining after the reaction is completed.

[0028] Preferably, the organic solvent is cyclohexane.

[0029] Preferably, the mass volume ratio of the cotton straw powder to anhydrous tin tetrachloride is 1g:15-20ml.

[0030] Preferably, after adding anhydrous tin tetrachloride, the reaction process is: stirring for 2-3 hours, standing for 24-26 hours, and stirring for 1 hour after sucking out the supernatant. In this reaction process, the reactants are first stirred to mix evenly, then standing for reaction, and after sucking out the supernatant that does not participate in the reaction, the stirring reaction is continued.

[0031] Preferably, the drying is vacuum drying at a temperature of 75-85° C. for 10-14 hours.

[0032] More preferably, the drying temperature is 80° C. and the drying time is 12 h.

[0033] Preferably, grinding is performed for 10-20 min.

[0034] Preferably, the calcination temperature is 600-800° C. and the calcination time is 1.5-2.5 h.

[0035] More preferably, the calcination temperature is 700° C. and the calcination time is 2 h.

[0036] The volume fraction of anhydrous tin tetrachloride used in the embodiment of the present invention is 98.2%-98.8%.

[0037] Example 1.

[0038] Sn-CS-Carbon-4 (1:20, referring to the mass volume ratio of cotton straw powder to cyclohexane is 1:20) was prepared. The specific steps are as follows:

[0039] (1) At room temperature, add 15.4 ml of cyclohexane to a 50 ml beaker, then add 0.2 g of cotton straw powder to the cyclohexane and stir for 30 min.

[0040] (2) 4 ml of anhydrous tin tetrachloride was added dropwise to the solution in step (1), stirred for 2 h, allowed to stand for 24 h, the supernatant was removed and stirred for 1 h, and the reaction was completed.

[0041] (3) The beaker was transferred to a vacuum drying oven and kept at 80°C for 12 h to obtain the precursor.

[0042] (4) After grinding the precursor for 10 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 700° C. at a rate of 5° C. / min, and the temperature was maintained at this temperature for 2 hours to obtain the tin-doped carbon composite material Sn-CS-Carbon-4.

[0043] Example 2.

[0044] Sn-CS-Carbon-3 (1:15, referring to the mass volume ratio of cotton straw powder to cyclohexane is 1:15) was prepared. The specific steps are as follows:

[0045] (1) At room temperature, add 15.4 ml of cyclohexane to a 50 ml beaker, then add 0.2 g of cotton straw powder to the cyclohexane and stir for 30 min.

[0046] (2) 3 ml of anhydrous tin tetrachloride was added dropwise to the solution in step (1), stirred for 2 h, allowed to stand for 24 h, the supernatant was removed and stirred for 1 h, and the reaction was completed.

[0047] (3) The beaker was transferred to a vacuum drying oven and kept at 80°C for 12 h to obtain the precursor.

[0048] (4) After grinding the precursor for 10 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 700° C. at a rate of 5° C. / min, and the temperature was maintained for 2 hours to obtain the tin-doped carbon composite material Sn-CS-Carbon-3.

[0049] Comparative Example 1.

[0050] Preparation of CS-Carbon: 0.2 g of cotton straw powder was placed in a 5 ml small crucible, and calcined at high temperature in a muffle furnace, with the temperature increased to 700° C. at a rate of 5° C. / min and maintained at the constant temperature for 2 h to obtain the carbon material CS-Carbon.

[0051] Example 3.

[0052] Sn-CS-Carbon-5 (1:25, referring to the mass volume ratio of cotton straw powder to cyclohexane is 1:25) was prepared. The specific steps are as follows:

[0053] (1) At room temperature, add 15.4 ml of cyclohexane to a 50 ml beaker, then add 0.2 g of cotton straw powder to the cyclohexane and stir for 30 min.

[0054] (2) Add 5 ml of anhydrous tin tetrachloride dropwise to the solution in step (1), stir for 2 h, let stand for 24 h, remove the supernatant and stir for 1 h, and the reaction is complete.

[0055] (3) The beaker was transferred to a vacuum drying oven and kept at 80°C for 12 h to obtain the precursor.

[0056] (4) After grinding the precursor for 10 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 700° C. at a rate of 5° C. / min, and the temperature was maintained at this temperature for 2 hours to obtain the tin-doped carbon composite material Sn-CS-Carbon-5.

[0057] Example 4.

[0058] The specific steps are as follows:

[0059] (1) At room temperature, add 40 ml of cyclohexane to a 100 ml beaker, then add 0.5 g of cotton straw powder into the cyclohexane and stir for 25 min.

[0060] (2) 10 ml of anhydrous tin tetrachloride was added dropwise to the solution in step (1), stirred for 3 h, allowed to stand for 24 h, the supernatant was removed and stirred for 1 h, and the reaction was completed.

[0061] (3) The beaker was transferred to a vacuum drying oven and kept at 75°C for 14 h to obtain the precursor.

[0062] (4) After grinding the precursor for 10 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 600°C at a rate of 5°C / min, and the temperature was maintained at this temperature for 2.5 hours to obtain a tin-doped carbon composite material.

[0063] Example 5.

[0064] The specific steps are as follows:

[0065] (1) At room temperature, add 50 ml of cyclohexane to a 100 ml beaker, then add 0.5 g of cotton straw powder into the cyclohexane and stir for 40 min.

[0066] (2) 8 ml of anhydrous tin tetrachloride was added dropwise to the solution in step (1), stirred for 3 h, allowed to stand for 26 h, the supernatant was removed and stirred for 1 h, and the reaction was completed.

[0067] (3) The beaker was transferred to a vacuum drying oven and kept at 85°C for 10 h to obtain the precursor.

[0068] (4) After grinding the precursor for 20 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 800°C at a rate of 5°C / min, and the temperature was maintained at this temperature for 1.5 hours to obtain a tin-doped carbon composite material.

[0069] Example 6.

[0070] The specific steps are as follows:

[0071] (1) At room temperature, add 18 ml of cyclohexane to a 50 ml beaker, then add 0.2 g of cotton straw powder into the cyclohexane and stir for 30 min.

[0072] (2) 4 ml of anhydrous tin tetrachloride was added dropwise to the solution in step (1), stirred for 3 h, allowed to stand for 26 h, the supernatant was removed and stirred for 1 h, and the reaction was completed.

[0073] (3) The beaker was transferred to a vacuum drying oven and kept at 83°C for 11 h to obtain the precursor.

[0074] (4) After grinding the precursor for 15 minutes, the precursor was placed in a muffle furnace for high-temperature calcination, the temperature was increased to 750°C at a rate of 5°C / min, and the temperature was maintained at this temperature for 2.0 hours to obtain a tin-doped carbon composite material.

[0075] Example 7.

[0076] The composite materials prepared in Examples 1, 2, 3 and Comparative Example 1 were used as negative electrode materials for lithium-ion batteries to assemble button batteries, and their electrical properties were tested.

[0077] (1) The test method is as follows:

[0078] The composite materials prepared in Examples 1, 2, 3 and Comparative Example 1 were used to prepare battery negative electrode materials. The active material (the composite materials prepared in Examples 1, 2, 3 and Comparative Example 1) and carbon black and binder polyvinylidene fluoride were mixed in nitrogen methyl pyrrolidone in a weight ratio of 8:1:1 to prepare three working electrodes. The mixture was then coated on copper foil and dried in a vacuum drying oven at 80°C for 12 h. After drying, the dried copper foil was cut into discs (10 mm) using a punching machine.

[0079] The button cell assembly was carried out in a glove box filled with argon. The CR2032 button cell was stacked and assembled in the order of "negative electrode shell, positive electrode, electrolyte, diaphragm, negative electrode, gasket, spring, positive electrode shell". Lithium hexafluorophosphate electrolyte was used as electrolyte and 16mm glass fiber diaphragm was used as diaphragm. After assembly, the button cell was packaged under a pressure of 5Mpa. The electrochemical performance of the assembled battery was tested after standing for 18 hours.

[0080] (2)Charge and discharge performance diagram

[0081] The results are shown in Table 1 and Figure 1-2 .

[0082] Figure 1 The tin-carbon negative electrode material prepared in Example 1 was -1 Charge and discharge performance diagram under current density. Figure 2 The carbon material prepared in Comparative Example 1 was -1 Charge and discharge performance diagram under current density. Figure 3 The tin-carbon negative electrode material prepared in Example 2 was -1 Charge and discharge performance diagram under current density. Figure 4 The tin-carbon negative electrode material prepared in Example 3 was -1 Charge and discharge performance diagram under current density.

[0083] The test results of the first coulombic efficiency and specific capacity are shown in Table 1.

[0084] Table 1

[0085]

[0086] Combined with Table 1, Figure 2 Display, at 50mA g -1 At the current density, the carbon material prepared in Comparative Example 1 exhibited a current of 1055.6 mAh·g -1 However, in the second cycle, the discharge capacity dropped rapidly to 445 mAh g -1 , and then stabilized, which was mainly due to the formation of SEI layer.

[0087] Combined with Table 1, Figure 1 The tin-carbon composite material prepared in Example 1 exhibited a capacity of 1118.6 mAh·g -1 The discharge capacity of the battery decreased to 627.9 mAh g in the second cycle. -1 , and then tended to be stable, and the specific capacity was much higher than that of the carbon material prepared in Comparative Example 1, indicating that the prepared tin-carbon negative electrode material has excellent lithium battery performance.

[0088] Combined with Table 1, Figure 1 , 3 4 show that the tin-carbon composite materials prepared in Examples 2 and 3 exhibited a capacity of 950.6 mAh·g -1 、1044.3mAh·g -1 The discharge capacity of the second cycle was reduced to 414 mAh g -1 、443.5mAh·g -1 , and then tended to be stable. The specific capacity of the two was much lower than that of the tin-carbon composite material prepared in Example 1. This may be due to the excessive increase in volume caused by excessive tin addition, which led to electrode cracking. This once again shows that the prepared tin-carbon negative electrode material has excellent lithium battery performance.

[0089] The above is only a preferred embodiment of the embodiment of the present invention, and does not impose any form of limitation on the embodiment of the present invention. Any simple modification, equivalent changes and modifications made to the above embodiment based on the technical essence of the embodiment of the present invention are still within the scope of the technical solution of the embodiment of the present invention.

Claims

1. A method for preparing an in-situ tin-doped carbon material, characterized in that: The preparation method comprises the following steps: adding cotton straw powder into an organic solvent, stirring and mixing evenly, adding anhydrous tin tetrachloride, and drying, grinding and calcining after the reaction is completed.

2. The preparation method according to claim 1, characterized in that: The organic solvent is cyclohexane.

3. The preparation method according to claim 1, characterized in that: The mass volume ratio of the cotton straw powder to anhydrous tin tetrachloride is 1g:15-20ml.

4. The preparation method according to claim 1, characterized in that: The drying is vacuum drying at a temperature of 75-85° C. for 10-14 hours.

5. The preparation method according to claim 4, characterized in that: The drying temperature is 80°C and the drying time is 12 hours.

6. The preparation method according to claim 1, characterized in that: The calcination temperature is 600-800°C and the calcination time is 1.5-2.5h.

7. The preparation method according to claim 6, characterized in that: The calcination temperature is 700° C. and the calcination time is 2 h.

8. A method for preparing an in-situ tin-doped carbon material, characterized in that: The in-situ tin-doped carbon material is prepared by the preparation method described in any one of claims 1-7.

9. Use of the in-situ tin-doped carbon material according to claim 8 in negative electrode materials for lithium-ion batteries.

Citation Information

Patent Citations

  • Stannous oxide / carbon composite material of lithium ion battery negative electrode and synthetic method of stannous oxide / carbon composite material

    CN108365207A

  • Method for preparing nano tin dioxide coated nitrogen-doped carbon composite material and application of nano tin dioxide coated nitrogen-doped carbon composite material