Boron-doped hard carbon negative electrode material and preparation method and application thereof
By doping boron elements and pore-forming treatment in hard carbon materials, combined with the use of amine catalysts, the problem of insufficient performance of hard carbon materials in battery applications is solved, the specific capacity and power performance are significantly improved, and the cycle stability is improved. properties and dynamic properties.
Patent Information
- Application Number
- CN202411052071.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-09-18
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-11
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In battery applications, hard carbon materials have problems such as high electrode potential, poor power performance, low initial efficiency, and low specific capacity. The high cost of raw materials limits their large-scale application.
By doping boron elements and performing pore-making processing, boron-doped hard carbon negative electrode materials are prepared to increase electronic conductivity and specific capacity. An amine catalyst is used to reduce the carbonization temperature, form more pores, and improve the electronic conductivity and cycle of the material. performance.
The specific capacity, first efficiency and power performance of hard carbon materials are significantly improved, the electrode potential is reduced, the cycle stability and kinetic properties of the material are improved, and the irreversible capacity is reduced.
Smart Images

Figure BDA0004975197730000051 
Figure BDA0004975197730000061 
Figure BDA0004975197730000062
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials, and specifically relates to a boron-doped hard carbon negative electrode material used for battery negative electrode materials. Background Art
[0002] Hard carbon is pyrolytic carbon of high molecular polymers, which is difficult to graphitize. It has an interlaced layered structure, which allows sodium ions to be embedded and released from all angles, thereby greatly improving the speed of charge and discharge. Compared with graphite materials, its low-temperature performance is also significantly improved, and hard carbon materials generally have a higher reversible specific capacity. However, hard carbon materials also often have disadvantages such as excessively high electrode potential, poor power performance, low initial efficiency, and low specific capacity. In addition, the raw materials generally come from biomass materials with low residual carbon content and high cost, which limits their large-scale application. Summary of the invention
[0003] In order to improve the specific capacity and power performance of hard carbon materials, the present invention prepares a boron-doped hard carbon negative electrode material by doping boron elements to improve the electronic conductivity and performing pore creation to improve the specific capacity.
[0004] The technical solution adopted by the present invention is as follows:
[0005] The technical purpose of the first aspect of the present invention is to provide a method for preparing a boron-doped hard carbon negative electrode material, comprising:
[0006] The coal-based asphalt, the boron-containing crosslinking agent, the pore-forming agent and the graphene are mixed under an inert atmosphere, placed in a reaction kettle at a temperature of 100-200° C. for crosslinking reaction, and the product is dried to obtain a hard carbon precursor composite material;
[0007] The hard carbon precursor composite material is heated to 200-500° C. and oxygen-containing gas is introduced to react to obtain a modified hard carbon material;
[0008] The modified hard carbon material and the amine catalyst are mixed, and heated and carbonized under an inert atmosphere to obtain a hard carbon composite material.
[0009] Furthermore, the weight ratio of the coal-based asphalt, the boron-containing crosslinking agent, the pore-forming agent and the graphene is 100:10-30:1-5:1-5. Before use, the coal-based asphalt is preferably crushed, preferably crushed to less than 100 μm; the pressure of the crosslinking reaction is 1-5 MPa, and the time is 1-6 hours. The drying is vacuum drying.
[0010] Furthermore, the boron-containing crosslinking agent is selected from at least one of trimethyl borate, triethyl borate, triisopropyl borate and diethylene glycol borate; the pore-forming agent is a wax, specifically, selected from at least one of paraffin wax, wood wax, rice bran wax and sugarcane wax.
[0011] Furthermore, the oxygen-containing gas is preferably a mixture of oxygen and an inert gas, which can be introduced after mixing or separately, and the volume ratio of oxygen to inert gas is 1:1-5. The time for introducing the oxygen-containing gas for oxidation reaction is 1-6h, and the total flow rate of the gas is 1-5L / min.
[0012] Furthermore, the modified hard carbon material and the amine catalyst are mixed in a weight ratio of 100:1-10.
[0013] Furthermore, the amine catalyst is selected from at least one of triethylamine, 4-dimethylaminopyridine, tetramethylguanidine and triethylenediamine.
[0014] Furthermore, the carbonization temperature is 1000-1300° C. and the time is 1-6 hours.
[0015] The technical purpose of the second aspect of the present invention is to provide a hard carbon negative electrode material prepared by the above preparation method.
[0016] The technical purpose of the second aspect of the present invention is to provide the application of the above-mentioned hard carbon negative electrode material as a battery negative electrode material, especially a sodium ion battery negative electrode material.
[0017] Implementing the embodiments of the present invention will have the following beneficial effects:
[0018] (1) The present invention dopes a boron crosslinking agent into a hard carbon precursor (coal-based asphalt). During the reaction, the boron crosslinking agent decomposes to produce boron free radicals, which crosslink with carbon and simultaneously form pores under the action of a pore-forming agent, thereby increasing specific capacity and electronic conductivity and improving power performance.
[0019] (2) The present invention uses oxygen-containing gas to heat treat the material after the cross-linking reaction, which can react with the hard carbon precursor composite material to form pores on the surface and shallow surface, thereby improving the sodium storage function of the material and bringing about an increase in specific surface area and an improvement in initial efficiency and specific capacity.
[0020] (3) The present invention selects an amine catalyst to mix with the modified hard carbon material and carbonizes it at a high temperature. The amine catalyst makes the reaction conditions milder to achieve carbonization and reduces the carbonization temperature (the carbonization temperature without adding an amine catalyst needs to be as high as 1500°C, and the carbonization temperature after adding an amine catalyst is 1000-1300°C). More pores can be formed to increase the specific capacity of the material, and nitrogen doping can be achieved during carbonization to improve the electronic conductivity of the material and improve the powder conductivity of the material. At the same time, the use of an amine catalyst can reduce material defects, reduce irreversible capacity, and improve the initial efficiency.
[0021] (4) The present invention dopes graphene into hard carbon to enhance the electronic conductivity and liquid retention performance of the material, improve the power and cycle performance, and add a catalyst to the modified hard carbon material during the carbonization process. DETAILED DESCRIPTION
[0022] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0023] Example 1
[0024] Step S1: 100g coal-based asphalt was crushed to about 50μm, then 20g trimethyl borate, 3g paraffin, and 3g graphene were added, stirred evenly, placed in a reactor at a pressure of 3Mpa and a temperature of 150°C for a cross-linking reaction for 3h, then filtered, and vacuum dried at 80°C for 24h to obtain a hard carbon precursor composite material;
[0025] Step S2: the hard carbon precursor composite material is transferred to a rotary kiln, the temperature is raised to 300° C., and a mixed gas of oxygen and argon (oxygen:argon volume ratio=1:3) is introduced, and the oxidation reaction is carried out for 3 hours at a mixed gas flow rate of 3 L / min to obtain a modified hard carbon material;
[0026] Step S3: 100 g of modified hard carbon and 5 g of triethylamine catalyst were mixed evenly, and then heated to 1200° C. in an argon inert atmosphere for carbonization for 3 h to obtain a hard carbon composite material.
[0027] Example 2
[0028] Step S1: Under an argon inert atmosphere, 100 g of coal-based asphalt was crushed to 50 μm, and then 10 g of triethyl borate, 1 g of wood wax, and 1 g of graphene were added, stirred evenly, placed in a reactor at a pressure of 1 MPa and a temperature of 100 ° C for a cross-linking reaction for 6 h, then filtered, and vacuum dried at 80 ° C for 24 h to obtain a hard carbon precursor composite material;
[0029] Step S2: the hard carbon precursor composite material is transferred to a rotary kiln, the temperature is raised to 200° C., and a mixed gas of oxygen and argon (oxygen:argon volume ratio=1:1) is introduced, and the oxidation reaction is carried out for 6 hours at a mixed gas flow rate of 5 L / min to obtain a modified hard carbon material;
[0030] Step S3: 100 g of modified hard carbon and 1 g of 4-dimethylaminopyridine catalyst are mixed evenly, and then heated to 1000° C. in an argon inert atmosphere for carbonization for 6 h to obtain a hard carbon composite material.
[0031] Example 3
[0032] Step S1: 100g coal-based asphalt was crushed to 50μm, then 30g triisopropyl borate, 5g rice bran wax, and 5g graphene were added, stirred evenly, placed in a reactor at a pressure of 5Mpa and a temperature of 200°C for a cross-linking reaction for 1h, then filtered, and vacuum dried at 80°C for 24h to obtain a hard carbon precursor composite material;
[0033] Step S2: the hard carbon precursor composite material is transferred to a rotary kiln, the temperature is raised to 500° C., and a mixed gas of oxygen and argon (oxygen:argon volume ratio=1:5) is introduced, and the oxidation reaction is carried out for 1 hour, and the mixed gas flow rate is 1 L / min to obtain a modified hard carbon material;
[0034] Step S3: 100 g of modified hard carbon and 10 g of tetramethylguanidine catalyst are mixed evenly, and then heated to 1300° C. in an argon inert atmosphere for carbonization for 1 h to obtain a hard carbon composite material.
[0035] Comparative Example 1
[0036] The difference from Example 1 is that trimethyl borate, paraffin and graphene are not added, and the other steps are the same as Example 1.
[0037] Comparative Example 2
[0038] The difference from Example 1 is that no triethylamine catalyst is added, and the other steps are the same as Example 1.
[0039] Comparative Example 3
[0040] The difference from Example 1 is that 20 g of boric acid is used instead of trimethyl borate, and the rest is the same as Example 1.
[0041] Comparative Example 4
[0042] The difference from Example 1 is that 10 g of boric acid and 10 g of furfural are used instead of trimethyl borate, and the rest is the same as Example 1.
[0043] Comparative Example 5
[0044] The difference from Example 1 is that oxygen is not added in step S2, and only argon gas with the same flow rate is used to replace the mixed gas. The rest is the same as Example 1.
[0045] Performance tests of the materials prepared in the above examples and comparative examples:
[0046] (1) Physical and chemical properties test:
[0047] According to the national standard GB / T-24533-2019 "Graphite Negative Electrode Materials for Lithium-ion Batteries", the specific surface area, tap density, particle size, powder conductivity, first discharge specific capacity and first charge and discharge efficiency of the hard carbon composite materials of the embodiments and comparative examples were tested; the test results are shown in Table 1.
[0048] Table 1
[0049]
[0050] It can be seen from Table 1 that the first discharge specific capacity, first charge and discharge efficiency, and specific surface area of the hard carbon composite materials obtained in Examples 1-3 are significantly better than those in the comparative example.
[0051] (2) Button battery
[0052] The hard carbon composite material obtained in the embodiment and the comparative example is used as the negative electrode (the mass ratio of the materials in the formula is hard carbon composite material: CMC: SBR: SP: H2O = 95: 2.5: 1.5: 1: 150), the lithium sheet is used as the positive electrode, the electrolyte is LiPF6 / EC+DEC (the volume ratio of the electrolyte solvent EC: DEC = 1: 1), the diaphragm is a composite film of polyethylene PE, polypropylene PP and polyethylene propylene PEP, and the button battery is assembled in an argon-filled glove box to assemble button batteries. The electrochemical performance is carried out on a Wuhan Landian CT2001A battery tester, the charge and discharge voltage range is controlled at 0.0-2V, the charge and discharge rate is 0.1C / 0.1C, and the 2C, 0.1C lithium removal capacity of the button battery, the DCR of the button battery and the cycle performance of the button battery (0.2C / 0.2C, 100 weeks) are tested at the same time; the test results are shown in Table 2.
[0053] Table 2
[0054]
[0055] It can be seen from Table 2 that the cycle performance and rate performance of the button cells made of the hard carbon composite materials of Examples 1-3 are significantly higher than those of the control example. The reason is that the hard carbon composite materials prepared by the present invention have high powder conductivity, reduce DCR, improve kinetic performance, improve rate performance, and can improve the cycle performance of the material.
[0056] (3) Soft pack battery
[0057] The hard carbon composite materials prepared in the embodiment and the comparative example were mixed and coated to prepare the negative electrode sheet, the ternary material NCM811 was used as the positive electrode, the solvent was EC / DEC / PC (volume ratio, EC:DEC:PC=1:1:1) as the electrolyte, the solute was LiPF6 (concentration of 1.3 mol / L), and the Celgard 2400 membrane was used as the separator, and 2Ah soft-pack batteries were prepared respectively.
[0058] Rate performance test:
[0059] The rate performance of the soft pack battery was tested with a charge and discharge voltage range of 2.75 to 4.2 V, a temperature of 25 ± 3.0 ° C, charging at 1.0 C, 3.0 C, 5.0 C, and 10.0 C, and discharging at 1.0 C. The test results of the rate performance constant current ratio are shown in Table 3.
[0060] Table 3
[0061]
[0062]
[0063] It can be seen from Table 3 that the rate charging performance of the soft-pack batteries in Examples 1-3 is significantly better than that in the comparative example, that is, the charging time is shorter. The reason for this is that boron is doped in the example materials to improve the electronic conductivity of the materials and improve the rate performance.
[0064] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a boron-doped hard carbon negative electrode material, comprising: The coal-based asphalt, the boron-containing crosslinking agent, the pore-forming agent and the graphene are mixed under an inert atmosphere, placed in a reaction kettle at a temperature of 100-200° C. for crosslinking reaction, and the product is dried to obtain a hard carbon precursor composite material; The hard carbon precursor composite material is heated to 200-500° C. and oxygen-containing gas is introduced to react to obtain a modified hard carbon material; The modified hard carbon material and the amine catalyst are mixed, and heated and carbonized under an inert atmosphere to obtain a hard carbon composite material.
2. The preparation method according to claim 1, characterized in that: The weight ratio of the coal-based asphalt, the boron-containing cross-linking agent, the pore-forming agent and the graphene is 100:10-30:1-5:1-5.
3. The preparation method according to claim 1, characterized in that: The pressure of the cross-linking reaction is 1-5Mpa, and the time is 1-6h.
4. The preparation method according to claim 1, characterized in that: The boron-containing cross-linking agent is selected from at least one of trimethyl borate, triethyl borate, triisopropyl borate and diethylene glycol borate; and the pore-forming agent is wax.
5. The preparation method according to claim 1, characterized in that: The oxygen-containing gas is a mixed gas with a volume ratio of oxygen to inert gas of 1:1-5. The time for introducing the oxygen-containing gas for oxidation reaction is 1-6 hours, and the total flow rate of the gas is 1-5 L / min.
6. The preparation method according to claim 1, characterized in that: The modified hard carbon material and the amine catalyst are mixed in a weight ratio of 100:1-10.
7. The preparation method according to claim 1, characterized in that: The amine catalyst is selected from at least one of triethylamine, 4-dimethylaminopyridine, tetramethylguanidine and triethylenediamine.
8. The preparation method according to claim 1, characterized in that: The carbonization temperature is 1000-1300° C. and the time is 1-6 hours.
9. A hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the hard carbon negative electrode material according to claim 9 as a negative electrode material for a battery.
Citation Information
Cited By
Preparation method and application of coal-based hard carbon negative electrode material
CN119911894A
Asphalt-based negative electrode material for sodium-ion battery and preparation method of asphalt-based negative electrode material
CN120767329A
A sodium-ion battery pitch-based anode material and its preparation method
CN120767329B
Preparation method and application of asphalt-based lithium ion battery hard carbon negative electrode coating material and negative electrode material
CN121123202A