Method for separating and purifying silicon carbide by taking industrial silicon smelting waste slag as raw material and application

Through crushing, wet grinding, interfacial modification flotation and ultrasonic centrifugation processes, the problem of separation and recovery of silicon carbide in industrial silicon smelting waste residue is solved, and efficient and high-purity silicon carbide recovery is achieved, which is suitable for the preparation of single crystal silicon carbide and waste residue. value-added utilization.

CN118754127AInactive Publication Date: 2024-10-11YUNNAN ENERGY RES INST CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410915650.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The basic phase characteristics and occurrence state of silicon carbide in industrial silicon smelting waste residue are unclear, resulting in no breakthrough in the separation and recovery process. It is necessary to develop a technology to realize the recovery and reuse of silicon carbide, which has economic and environmental value.

Method used

Through crushing, wet grinding, interface modification flotation and ultrasonic centrifugation processes, silicon carbide is separated and purified to achieve uniform particle size, concentrated particle distribution, regular morphology and high purity recovery of silicon carbide without waste gas emissions.

Benefits of technology

It achieves efficient recovery of silicon carbide from industrial silicon smelting waste residue, is suitable for the preparation of single crystal silicon carbide, has great industrialization prospects, and realizes the value-added utilization of waste residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754127A_ABST
    Figure CN118754127A_ABST
Patent Text Reader

Abstract

The invention discloses a method for separating and purifying silicon carbide by taking industrial silicon smelting waste slag as a raw material and application, and belongs to the technical field of industrial silicon smelting waste slag recovery. The specific preparation method comprises the following steps: (1) crushing the industrial silicon smelting waste residue, performing wet grinding, adding a wet-ground material into a flotation tank, and performing flotation to obtain flotation concentrate; and (2) carrying out acid leaching on the flotation concentrate, then carrying out ultrasonic treatment, carrying out centrifugal separation on the powder subjected to ultrasonic treatment, and filtering and drying precipitates in a centrifugal tube to obtain silicon carbide powder. The method is simple in operation process, free of environmental pollution and obvious in separation effect; the method is applied to recycling of the industrial silicon smelting waste residues, the recycled silicon carbide particles are uniform in particle size and concentrated in particle distribution, the recycled silicon carbide particles can be used for preparing single crystal silicon carbide wafers in the next step, and a feasible development direction is provided for industrial production of recycling silicon carbide powder from the industrial silicon smelting waste residues; and a feasible development direction is provided for the application of the recycled silicon carbide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for separating and purifying silicon carbide by taking industrial silicon smelting waste slag as raw material and application thereof, belonging to the field of recycling and utilizing industrial silicon smelting waste slag. Background Art

[0002] SiC silicon carbide is one of the ideal materials for making high-temperature, high-frequency, high-power, and high-voltage devices. Compared with traditional silicon materials (Si), the core advantages of silicon carbide raw materials are reflected in: high-voltage resistance, lower impedance, wider bandgap, and the ability to withstand larger currents and voltages, resulting in smaller product designs and higher efficiency; high-frequency resistance, SiC devices do not have current tailing during the shutdown process, which can effectively increase the switching speed of components (about 3-10 times that of Si), and are suitable for higher frequencies and faster switching speeds; high-temperature resistance, SiC has higher thermal conductivity than silicon and can work at higher temperatures.

[0003] According to the application characteristics of silicon carbide in different fields, it can be divided into high-purity silicon carbide (HP-SiC), industrial-grade silicon carbide (RP-SiC), etc.; industrial-grade silicon carbide has good corrosion resistance and high temperature resistance, and is suitable for the manufacture of chemical equipment and refractory materials.

[0004] The basic phase characteristics and occurrence state of silicon carbide in industrial silicon smelting waste slag are not clear, resulting in no breakthrough in the process of separating and recovering silicon carbide from industrial silicon smelting waste slag. Therefore, it is necessary to develop a technology for recovering silicon carbide from industrial silicon smelting waste slag to achieve the recovery and reuse of silicon carbide in industrial silicon smelting waste slag, which has considerable economic and environmental value. Summary of the invention

[0005] The purpose of the present invention is to provide a method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, and to obtain industrial silicon smelting waste slag material meeting a certain particle size through a flotation-centrifugation process; in addition, the recovered silicon carbide material has uniform particle size, concentrated particle distribution, regular morphology and high purity, and no waste gas emissions, and is applied to the preparation of single-crystal silicon carbide, with great industrial prospects.

[0006] The technical solution of the present invention is as follows, which specifically comprises the following steps:

[0007] (1) The raw material block industrial silicon smelting waste slag is crushed and classified to screen the fine industrial silicon smelting waste slag.

[0008] (2) fine particles of industrial silicon smelting waste slag are wet-ground, and the industrial silicon smelting waste slag solution after wet grinding is added to the flotation tank for interface modification flotation, and the flotation concentrate is simply acid-leached and dried at a constant temperature to obtain fine powder of industrial silicon smelting waste slag.

[0009] (3) The dried industrial silicon smelting waste slag fine powder is added to a heavy liquid for ultrasonic treatment and centrifugal separation to obtain silicon carbide particles.

[0010] Furthermore, the crusher in step S1 is one or more of a jaw crusher, a cone crusher, an impact crusher, a gyratory crusher and a roll crusher.

[0011] Furthermore, the fine particles screened in step S1 have a particle size of 1 mm to 100 μm.

[0012] Furthermore, the concentration of the industrial silicon smelting waste slag slurry after wet grinding in step S2 is 40-80%.

[0013] Furthermore, the inhibitor added for the interfacial modification in step S2 is one or more of water glass, PAM, SHMP, PEG, sodium carboxymethyl cellulose, starch, sodium metaphosphate and thioacid salt, and the added amount of the inhibitor is 100-1000 g / t.

[0014] Furthermore, the collector added for the interface modification in step S2 is one or more of No. 2 oil, oleic acid, kerosene, xanthate, OP-10, and fatty amine, and the added amount of the collector is 100-1000 g / t.

[0015] Furthermore, in step S2, the acid leaching solution is one or more of hydrochloric acid, nitric acid, hypochlorous acid, perchloric acid, and hydrofluoric acid, the concentration of the acid leaching solution is 1-6 mol / L, and the solid-liquid ratio of the added flotation concentrate to the acid leaching solution is 1:(10-80), in units of g:ml.

[0016] Furthermore, in step S3, the solid-liquid ratio of the dried industrial silicon smelting waste slag fine powder and the heavy liquid is 1:(10-50), and the ultrasonic time of the mixed solution is 1-60 min.

[0017] Furthermore, in step S3, the rotation speed of the centrifugal separation is 5000-15000 r / min, the centrifugal time is 1-15 min, and the number of centrifugation times is 1-5 times.

[0018] Another object of the present invention is to provide a method and application of recovering silicon carbide material using industrial silicon smelting waste slag as raw material; using cheap industrial silicon smelting waste slag to prepare silicon carbide realizes the value-added utilization of the waste slag.

[0019] The principle of the present invention is as follows: the industrial silicon smelting waste slag is subjected to a simple crushing and wet grinding process to achieve the dissociation of silicon carbide in the industrial silicon smelting waste slag, and the content of silicon carbide is further increased through the flotation industry according to the interface physical properties of silicon carbide, which is conducive to the subsequent centrifugal process to better separate silicon carbide from other phases according to the different physical properties, thereby achieving the separation, recovery and purification of silicon carbide in the industrial silicon smelting waste slag.

[0020] The beneficial effects of the present invention are:

[0021] (1) Industrial silicon smelting waste slag can achieve the effect of silicon carbide dissociation through simple crushing and wet grinding processes, and flotation process is selected for preliminary separation of silicon carbide; the above-mentioned crushing, wet grinding and flotation processes can all be realized on a large scale industrially.

[0022] (2) The reagents selected in the flotation process can effectively separate silicon carbide. According to the interface modification in the flotation process, the selected reagents do not affect the basic properties of silicon carbide.

[0023] (3) With regard to the selection of wet grinding-flotation combined with centrifugal process for separating silicon carbide, the pH of the slurry changes during the wet grinding process, and this pH change is beneficial to the flotation experiment; the particle size obtained by the wet grinding-flotation process can better meet the subsequent centrifugal separation of silicon carbide. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a schematic flow chart of the invention for recovering silicon carbide from industrial silicon smelting waste slag.

[0025] Figure 2 This is the XRD diagram of silicon carbide recovered in Example 1 of the present invention.

[0026] Figure 3 This is a SEM image of the silicon carbide recovered in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The present invention is further described below in conjunction with specific examples, but the present invention is not limited to the following examples. The experimental methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.

[0028] Example 1

[0029] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0030] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm.

[0031] (2) Fine particles of industrial silicon smelting waste slag are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 50%. 300 g / t of inhibitor sodium silicate and 200 g / t of collector No. 2 oil are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 2 mol / L hydrochloric acid and dried at a constant temperature to obtain fine powder of industrial silicon smelting waste slag, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:50, and the unit is g:ml.

[0032] (3) The dried industrial silicon smelting waste slag powder was added with bromoform (containing 10% deionized water) at a solid-liquid ratio of 1:20, and subjected to ultrasonic treatment for 5 minutes. The powder was centrifuged at a speed of 5000 r / min for 5 minutes, and centrifuged twice to obtain silicon carbide particles. The XRD pattern of the silicon carbide particles obtained in this example is shown in FIG. Figure 1 As shown in the figure, it can be seen that the material after centrifugal separation is mainly silicon carbide, and the characteristic peak of silicon carbide is particularly obvious. The SEM picture is as follows Figure 2 As shown in the figure, it can be seen that the silicon carbide obtained by separating and recovering industrial silicon smelting waste slag is in flaky form and the particles are tightly combined.

[0033] The purity of the silicon carbide obtained in this example is 99.2%, and the recovery rate reaches 90%.

[0034] Example 2

[0035] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0036] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm;

[0037] (2) Fine particles of industrial silicon smelting waste slag are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 50%. 300 g / t of inhibitor sodium silicate and 300 g / t of collector oleic acid are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 2 mol / L hydrochloric acid and dried at a constant temperature to obtain fine powder of industrial silicon smelting waste slag, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:50, and the unit is g:ml.

[0038] (3) The dried industrial silicon smelting waste slag fine powder was added with iodomethane (containing 20% ​​deionized water) at a solid-liquid ratio of 1:25, and ultrasonic treatment was performed for 15 minutes. The mixture was centrifuged at a speed of 15000 r / min for 5 minutes, and the centrifugation was performed twice to obtain silicon carbide particles.

[0039] The purity of the silicon carbide obtained in this embodiment is 90.8%, and the recovery rate is 88%.

[0040] Example 3

[0041] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0042] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm.

[0043] (2) Fine particles of industrial silicon smelting waste slag are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 70%. 500 g / t of inhibitor sodium silicate and 100 g / t of frother No. 2 oil are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 3 mol / L hydrochloric acid and dried at a constant temperature to obtain fine powder of industrial silicon smelting waste slag, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:30, and the unit is g:ml.

[0044] (3) The dried industrial silicon smelting waste slag fine powder was added to Song's heavy liquid (containing 20% ​​deionized water) at a solid-liquid ratio of 1:15, and ultrasonic treatment was performed for 15 minutes. The powder was centrifuged at a speed of 5000 r / min for 5 minutes, and the centrifugation was performed twice to obtain silicon carbide particles.

[0045] The purity of the silicon carbide obtained in this embodiment is 88.5%, and the recovery rate is 84%.

[0046] Example 4

[0047] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0048] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm.

[0049] (2) Fine particles of industrial silicon smelting waste slag are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 60%. 200 g / t of inhibitor sodium silicate and 500 g / t of collector oleic acid are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 6 mol / L hydrochloric acid and dried at a constant temperature to obtain fine powder of industrial silicon smelting waste slag, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:50, and the unit is g:ml.

[0050] (3) The dried industrial silicon smelting waste slag powder was added to Kjeldahl heavy liquid (containing 20% ​​deionized water) at a solid-liquid ratio of 1:25, and ultrasonic treatment was performed for 15 minutes. The powder was centrifuged at a speed of 5000 r / min for 5 minutes, and the centrifugation was performed twice to obtain silicon carbide particles.

[0051] The purity of the silicon carbide obtained in this embodiment is 90.5%, and the recovery rate is 86%.

[0052] Example 5

[0053] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0054] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm.

[0055] (2) The industrial silicon smelting waste slag particles are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 70%. 600 g / t of inhibitor sodium silicate and 500 g / t of collector No. 2 oil are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 4 mol / L hydrochloric acid and dried at a constant temperature to obtain industrial silicon smelting waste slag fine powder, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:60, and the unit is g:ml.

[0056] (3) The dried industrial silicon smelting waste slag powder was added to Kjeldahl heavy liquid (containing 40% deionized water) at a solid-liquid ratio of 1:20, and ultrasonic treatment was performed for 15 minutes. The powder was centrifuged at a speed of 2000 r / min for 5 minutes, and the centrifugation was repeated twice to obtain silicon carbide particles.

[0057] The purity of the silicon carbide obtained in this embodiment is 86.5%, and the recovery rate is 89%.

[0058] Example 6

[0059] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0060] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 1 mm.

[0061] (2) The industrial silicon smelting waste slag particles are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 80%. 300 g / t of inhibitor sodium silicate and 300 g / t of collector oleic acid are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 6 mol / L hydrochloric acid and dried at a constant temperature to obtain industrial silicon smelting waste slag fine powder, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:80, and the unit is g:ml.

[0062] (3) The dried industrial silicon smelting waste slag powder was added to Song's heavy liquid (containing 50% deionized water) at a solid-liquid ratio of 1:50, and ultrasonic treatment was performed for 25 minutes. The powder was centrifuged at a speed of 15000 r / min for 5 minutes, and the centrifugation was performed twice to obtain silicon carbide particles.

[0063] The purity of the silicon carbide obtained in this embodiment is 88.5%, and the recovery rate is 89%.

[0064] Example 7

[0065] A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, specifically comprising the following steps:

[0066] (1) The raw material block industrial silicon smelting waste slag is crushed and classified by a jaw crusher to screen the industrial silicon smelting waste slag with a particle size of 5 mm.

[0067] (2) The industrial silicon smelting waste slag particles are wet-grinded by a rod mill. The concentration of the industrial silicon smelting waste slag solution after wet grinding is 50%. 300 g / t of sodium silicate inhibitor and 200 g / t of No. 2 oil frother are added to the flotation tank for interface modification flotation. The flotation concentrate is acid-leached with 2 mol / L hydrochloric acid and dried at a constant temperature to obtain industrial silicon smelting waste slag fine powder, wherein the solid-liquid ratio of the flotation concentrate to the acid-leaching solution is 1:10, and the unit is g:ml.

[0068] (3) The dried industrial silicon smelting waste slag fine powder was added with methyl bromide (containing 30% deionized water) at a solid-liquid ratio of 1:20, and ultrasonic treatment was performed for 15 minutes. The mixture was centrifuged at a speed of 10,000 r / min for 5 minutes, and centrifuged twice to obtain silicon carbide particles.

[0069] The purity of the silicon carbide obtained in this embodiment is 96.6%, and the recovery rate is 91%.

[0070] The above is a further detailed description of the present invention in combination with a specific implementation method, and does not impose any formal limitations on the present invention; for ordinary technicians in the technical field and industry to which the present invention belongs, they can make some simple deductions or replacements without departing from the concept of the present invention; at the same time, any modification, replacement and replacement of the above embodiments according to the essential technology of the present invention are within the protection scope of the technology of the present invention.

Claims

1. A method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material, characterized in that: The method comprises the following preparation steps: (1) The raw material block industrial silicon smelting waste slag is crushed and classified to screen fine particles; (2) Wet-grinding fine particles of industrial silicon smelting waste slag, adding the wet-grinded industrial silicon smelting waste slag solution into a flotation tank for interface modification flotation, acid-leaching the flotation concentrate and drying at a constant temperature to obtain industrial silicon smelting waste slag fine powder; (3) The dried industrial silicon smelting waste slag fine powder is added to heavy liquid for ultrasonic treatment and centrifugal separation to obtain silicon carbide particles.

2. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: The fine particles screened in step (1) have a particle size of 1 mm to 100 μm.

3. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: In step (2), the concentration of the industrial silicon smelting waste slag slurry after wet grinding is 40-80%.

4. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: In step (2), the inhibitor added for interfacial modification flotation is one or more of water glass, PAM, SHMP, PEG, sodium carboxymethyl cellulose, starch, sodium metaphosphate and thioacid salt, and the added amount of the inhibitor is 100-1000g / t.

5. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: The collector added for interface modification in step (2) is one or more of No. 2 oil, oleic acid, kerosene, xanthate, OP-10, and fatty amine, and the amount of the collector added is 100-1000 g / t.

6. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: In step (2), the acid leaching solution is one or more of hydrochloric acid, nitric acid, hypochlorous acid, perchloric acid, and hydrofluoric acid, with a concentration of 1-6 mol / L. The solid-liquid ratio of the added flotation concentrate to the acid leaching solution is 1:(10-80), in units of g:ml.

7. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: During the ultrasonic treatment in step (3), the solid-liquid ratio of the dried industrial silicon smelting waste slag fine powder to the heavy liquid is 1:(10-50), in units of g:ml, and the ultrasonic treatment time of the mixed solution is 1-60min.

8. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: In step (3), the rotation speed of the centrifugal separation is 5000-15000 r / min, the centrifugal time is 1-15 min, and the number of centrifugation is 1-5 times.

9. The method for separating and purifying silicon carbide using industrial silicon smelting waste slag as raw material as claimed in claim 1, characterized in that: The heavy liquid in step (3) is obtained by adding 1% to 50% by mass of deionized water to one or more of bromoform, dibromoform, tetrabromoethane, Dullerian solution, diiodomethane, tin tetrabromide, tribromofret, and Klein's heavy liquid.

10. Use of the method according to any one of claims 1 to 9 in recycling silicon carbide.

Citation Information

Patent Citations

  • Method for preparing silicon carbide powder from polycrystalline silicon cutting wastes

    CN105293498A

  • Heavy liquid for separating silicon and silicon carbide and separation method for silicon and silicon carbide

    CN106966396A

  • Preparation method for silicon carbide micropowder for fine silicon carbide ceramic

    CN108752003A