Preparation method of petal-shaped antimony trioxide
By adopting the preparation method of petal-shaped antimony trioxide in lithium-ion batteries, alcohol solvent and morphology control agent are used to generate antimony trioxide particles with petal-like structure, which solves the problem of volume expansion and agglomeration of Sb2O3 in lithium-ion batteries. problem, achieving excellent electrochemical performance and cycling stability.
Patent Information
- Application Number
- CN202410851509.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Sb2O3 has problems with volume expansion, material powdering and agglomeration during the charge and discharge process of lithium-ion batteries, which affects its cycle performance.
Using the preparation method of petal-like antimony trioxide, by adding antimony salt, morphology control agent and pH control agent to the alcohol solvent, a solvothermal reaction is performed to generate antimony trioxide particles with a petal-like structure, using polyvinylpyrrole Enone and diethylene glycol ether protect the particles, avoid agglomeration and promote directional growth.
The formed petal-like antimony trioxide has excellent electrochemical properties, especially good cycle stability, slows down the volume expansion during charge and discharge, and improves conductivity and charge storage capacity.
Smart Images

Figure CN118754196A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of inorganic materials, and in particular to a method for preparing petal-shaped antimony trioxide. Background Art
[0002] In recent years, lithium-ion batteries have been widely used as an important part of the power systems of mobile devices, electric vehicles, aerospace and other equipment. Sb2O3 has a high theoretical capacity, low price, abundant reserves, and relatively stable cycle performance. It is a very promising electrode material, but Sb2O3 has a large volume expansion during the charge and discharge process. During the cycle, the repeated insertion and extraction of lithium ions causes the material to pulverize and agglomerate, which seriously hinders its practical application. Summary of the invention
[0003] Purpose of the invention: In view of the above technical problems, the present invention proposes a method for preparing petal-shaped antimony trioxide.
[0004] The technical solutions adopted are as follows:
[0005] A method for preparing petal-shaped antimony trioxide:
[0006] Add antimony salt to alcohol solvent, heat to 40-50°C and keep stirring for 30-60 minutes, then add morphology control agent and pH control agent, and finally subject the obtained reaction solution to solvent thermal reaction, collect the precipitate, wash and dry it.
[0007] Furthermore, the antimony salt is any one or more combinations of antimony chloride, antimony sulfate and antimony nitrate.
[0008] Furthermore, the antimony salt is antimony chloride.
[0009] Furthermore, the alcohol solvent is any one or more combinations of ethanol, ethylene glycol, n-propanol, isopropanol, propylene glycol, and glycerol.
[0010] Furthermore, the morphology control agent includes diethylene glycol ether and polyvinyl pyrrolidone.
[0011] Furthermore, the mass ratio of diethylene glycol ether to polyvinyl pyrrolidone is 1-5:1-5.
[0012] Furthermore, the mass ratio of the morphology control agent to the antimony salt is 0.1-1:1.
[0013] Furthermore, the pH control agent is hexamethylenetetramine and / or urea.
[0014] Furthermore, the temperature of the solvothermal reaction is 120-160°C.
[0015] Furthermore, the solvent thermal reaction time is 1-10h.
[0016] Beneficial effects of the present invention:
[0017] The present invention provides a method for preparing petal-shaped antimony trioxide. The alcohol solvent is both a solvent and a reactant. The antimony salt reacts with the alcohol solvent to generate an antimony alkoxide precursor. At high temperature, the pH control agent slowly decomposes to generate OH - Under the action of the morphology control agent, the antimony alkoxide precursor decomposes and continues to grow to form antimony trioxide particles with a petal-like structure. In the early stage of the decomposition of the antimony alkoxide precursor crystal nucleus, the generated antimony trioxide grains have a high surface free energy and are very easy to agglomerate to form secondary particles. Polyvinyl pyrrolidone can protect them at the moment of nucleation, effectively avoiding secondary growth or agglomeration. The hydroxyl functional groups on diethylene glycol ether are conducive to the formation of Sb 3+ The adsorption nucleation of ions enables the subsequently generated antimony trioxide to be directionally and stably dispersed and grown on the outer surface of the antimony trioxide grains, and finally forms a special petal-like morphology. The antimony trioxide prepared by the present invention has excellent electrochemical properties, especially good cycle stability. The reason may be that the special petal-like morphology can store more charges and ions, and can also provide more transmission channels for them, thereby improving the conductivity of antimony trioxide and slowing down the volume expansion during the charge and discharge process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 This is the TEM image of the petal-shaped antimony trioxide prepared in Example 1.
[0019] Figure 2 This is the SEM image of antimony trioxide prepared in Comparative Example 1.
[0020] Figure 3 This is the SEM image of antimony trioxide prepared in Comparative Example 2. DETAILED DESCRIPTION
[0021] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially. The techniques not mentioned in the present invention are all referenced to the prior art. Unless otherwise specified, the following examples and comparative examples are parallel experiments, using the same processing steps and parameters.
[0022] Embodiment 1:
[0023] A method for preparing petal-shaped antimony trioxide:
[0024] Add 5g of antimony chloride to 300ml of isopropanol and mix well. Heat to 45℃ and keep stirring for 60min. Then add 1g of diethylene glycol ether, 1g of polyvinyl pyrrolidone and 23g of urotropine. Stir well to obtain a reaction solution. Seal the reaction solution in an autoclave and heat to 150℃ for 5h. Cool naturally to room temperature and collect the precipitate. Wash with deionized water and ethanol in turn. Finally, dry in an oven at 80℃ for 10h. Figure 1 The microscopic morphology is petal-shaped, the size is uniform, and the purity is ≥99.9%.
[0025] Embodiment 2:
[0026] A method for preparing petal-shaped antimony trioxide:
[0027] 5g of antimony chloride was added to 300ml of isopropanol and mixed, heated to 45℃ and stirred for 60min, then 0.5g of diethylene glycol ether, 0.5g of polyvinyl pyrrolidone and 23g of urotropine were added, and the reaction liquid was obtained after sufficient stirring. The reaction liquid was sealed in a high-pressure reactor and heated to 140℃ for 8h. After natural cooling and returning to room temperature, the precipitate was collected and washed with deionized water and ethanol in turn, and finally dried in an oven at 80℃ for 10h. The microscopic morphology was petal-shaped, the size was uniform, and the purity was ≥99.9%. .
[0028] Embodiment 3:
[0029] A method for preparing petal-shaped antimony trioxide:
[0030] 5 g of antimony chloride was added to 300 ml of isopropanol and mixed, the temperature was raised to 45° C. and the mixture was stirred for 60 min. Then 1 g of diethylene glycol ether, 0.5 g of polyvinyl pyrrolidone and 23 g of urotropine were added and the mixture was stirred thoroughly to obtain a reaction solution. The reaction solution was sealed in a high-pressure reactor and heated to 160° C. for reaction for 10 h. After natural cooling and recovery to room temperature, the precipitate was collected and washed with deionized water and ethanol in turn, and finally dried in an oven at 80° C. for 10 h. The microscopic morphology was petal-shaped, the size was uniform, and the purity was ≥99.9%.
[0031] Comparative Example 1:
[0032] The same as Example 1, except that no diethylene glycol ether was added. Figure 2 The microscopic morphology is irregular agglomerates, and the purity is ≥99.9%.
[0033] Comparative Example 2:
[0034] The same as Example 1, except that polyvinyl pyrrolidone was not added. Figure 3 The microscopic morphology is disc-shaped and the purity is ≥99.9%.
[0035] Performance Test:
[0036] The antimony trioxide prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 is respectively used as an active material, N-methyl-2-pyrrolidone is used as a solvent, polyvinylidene fluoride (PVDF) is used as a binder, and acetylene black is used as a conductive agent. The active material, the binder, and the conductive agent are weighed in a mass ratio of 8:1:1. First, the binder is fully dissolved in the solvent in a weighing bottle, and then the mixture of acetylene black and the active material is slowly added. The slurry obtained by stirring is coated on a clean copper foil with a coating machine. The coated copper foil is placed in a vacuum drying oven and dried at 100°C for 24 hours. It is taken out and punched into a circular negative electrode sample with a diameter of 14 mm by a slicer. The sample is placed in a glove box protected by a high argon atmosphere. The sample is used as a working electrode, and the metal lithium sheet is used as a positive electrode sheet. LiPF6 / ethylene carbonated (EC) / dimenthyl Carbonate (DEC) is used as the electrolyte, polypropylene is used as the separator, and a CR2025 button cell is assembled. The battery is assembled in the order of negative electrode cover, negative electrode sheet, electrolyte, separator, electrolyte, positive electrode sheet, gasket, and positive electrode cover. The assembled battery is taken out of the glove box, and the positive and negative electrode shells are pressed and sealed with a sealing machine to obtain a CR2025 button cell. The electrochemical performance test is tested by the blue power test system. It is activated for three cycles at a small rate of 0.1C, and then transferred to 1C conditions for charge and discharge cycle test. The test results are shown in Table 1 below:
[0037] Table 1:
[0038]
[0039] As can be seen from Table 1 above, the antimony trioxide prepared by the present invention has excellent electrochemical properties, especially good cycle stability. The reason may be that the special petal-shaped morphology can store more charges and ions, and can also provide more transmission channels for them, thereby improving the conductivity of antimony trioxide and slowing down the volume expansion during the charge and discharge process.
[0040] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing petal-shaped antimony trioxide, characterized in that: Add antimony salt to alcohol solvent, heat to 40-50°C and keep stirring for 30-60 minutes, then add morphology control agent and pH control agent, and finally subject the obtained reaction solution to solvent thermal reaction, collect the precipitate, wash and dry it.
2. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The antimony salt is any one or more combinations of antimony chloride, antimony sulfate and antimony nitrate.
3. The method for preparing petal-shaped antimony trioxide according to claim 2, characterized in that: The antimony salt is antimony chloride.
4. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The alcohol solvent is any one or more combinations of ethanol, ethylene glycol, n-propanol, isopropanol, propylene glycol, and glycerol.
5. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The morphology control agent includes diethylene glycol ether and polyvinyl pyrrolidone.
6. The method for preparing petal-shaped antimony trioxide according to claim 5, characterized in that: The mass ratio of the diethylene glycol ether to the polyvinyl pyrrolidone is 1-5:1-5.
7. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The mass ratio of the morphology control agent to the antimony salt is 0.1-1:
1.
8. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The pH control agent is hexamethylenetetramine and / or urea.
9. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The temperature of the solvothermal reaction is 120-160°C.
10. The method for preparing petal-shaped antimony trioxide according to claim 1, characterized in that: The solvent thermal reaction time is 1-10h.
Citation Information
Patent Citations
Preparation method of bowknot-shaped antimonous oxide
CN102167399A
Preparation method and application of antimonous oxide different in features
CN102659179A
Preparation method of nano antimony trioxide
CN108557883A
Antimony trioxide applied to negative electrode materials for lithium ion batteries and method for preparing antimony trioxide
CN108706633A