Method for catalytic degradation of dye wastewater by photocatalysis cooperating with Fenton-like reaction
Fe3O4-TiO2 magnetic nanosheet photocatalysis synergistic Fenton-like reaction system solves the problems of low efficiency and high cost in dye wastewater treatment, achieves efficient degradation of RhB dye and multiple reuse of catalysts, significantly improving treatment efficiency and stability.
Patent Information
- Application Number
- CN202410793598.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The existing technology has low efficiency, high cost and easy secondary pollution when treating dye wastewater. In particular, rhodamine B (RhB) dye has poor biodegradability and has potential risks of mutagenesis and carcinogenesis, making it difficult to achieve efficient, fast and low-cost treatment. degradation.
Fe3O4-TiO2 magnetic nanosheets are used as the photocatalytic synergistic Fenton-like reaction system. They are prepared through steps such as heat treatment and ultrasound. They are combined with H2O2 for catalytic degradation under light. The chemical bond between Fe3O4 and TiO2 is used to improve the catalytic activity, and multiple magnetic separations are achieved through magnetic separation. reused.
Efficient and rapid degradation of RhB dye was achieved, with a catalytic degradation rate and recovery rate exceeding 90%, reducing costs and significantly improving the reusability and stability of the catalyst.
Smart Images

Figure HDA0004900806590000011 
Figure HDA0004900806590000012 
Figure HDA0004900806590000013
Abstract
Description
Technical Field
[0001] The invention relates to a method for photocatalytically cooperating with Fenton-like reaction to catalyze and degrade dye wastewater, belonging to the technical field of environmental engineering / inorganic functional materials and photocatalytic wastewater treatment. Background Art
[0002] Water is the source of life and plays an irreplaceable role in the survival of humans and all living things. However, with the rapid development of the global economy and industrialization, water pollution has become increasingly serious, among which organic pollutants such as organic dyes, benzene compounds, and phenolic compounds have become the main sources of pollution. In the textile, papermaking and other industries, dyes are indispensable compounds. It is worth noting that rhodamine B (RhB) has become an important source of organic pollutants in dye wastewater due to its wide application. The strong coloring properties of RhB not only hinder the penetration of sunlight, reduce the dissolved oxygen content in water, and thus affect the photosynthesis and normal growth of plants, but also destroy the balance of water ecology. In addition, the organic pollutants in RhB dye wastewater have poor biodegradability and have potential risks of mutagenesis, carcinogenesis and teratogenesis. Therefore, in order to achieve efficient, rapid and low-cost degradation of RhB dye wastewater, the development of new and efficient catalysts and the construction of efficient catalytic systems have become major issues that need to be solved urgently.
[0003] Although biological methods, adsorption methods, chemical oxidation methods, etc. have been applied to treat wastewater containing dyes, these methods still face many challenges in practical applications due to problems such as low efficiency, high cost, and easy secondary pollution. Advanced oxidation processes (AOPs) can degrade organic pollutants into non-toxic and harmless substances such as CO2, H2O, and inorganic salts, and have become the focus of research in recent years. Among them, Fenton oxidation and photocatalytic oxidation have attracted much attention due to their mild process reaction conditions, simple operation, and good pollutant removal effects. In addition, the effective combination of the two oxidation processes to construct an efficient catalytic oxidation system can further improve the catalytic degradation effect of organic pollutants in wastewater. At present, most researchers combine the photocatalyst TiO2 with the Fenton-like catalyst Fe3O4. The photogenerated e - Can be transferred to Fe 3+ On the Fe 3+ / Fe 2+ The conversion rate of photogenerated e in TiO2 is inhibited - -h +The combination of Fe3O4 and Fe3O4 produces more active species, which catalyzes the oxidation and degradation of organic pollutants. However, ordinary Fe3O4 magnetic nanoparticles have defects such as easy recombination of carriers and easy aggregation in solution, which seriously affect the catalytic activity. In recent years, two-dimensional transition metal oxides have shown good application prospects in electrocatalysis, electronic devices and energy storage due to their inherent quantum confinement of electrons. The unique two-dimensional nanostructure of Fe3O4 nanosheets exposes more active sites, which is not only conducive to the deposition and loading of TiO2 nanoparticles, but also has a faster electron transfer rate, providing great opportunities for the development of new and efficient catalysts and catalytic degradation methods. Summary of the invention
[0004] The purpose of the present invention is to provide a method for catalytic degradation of dye wastewater by photocatalysis and Fenton-like reaction. The present invention applies a magnetically recoverable Fe3O4-TiO2 photocatalytic synergistic Fenton-like reaction system to the catalytic degradation of RhB dye wastewater. The application of Fe3O4-TiO2 nanosheets not only realizes the efficient degradation of RhB dye wastewater, but also can be reused multiple times, significantly reducing costs.
[0005] The Fe3O4-TiO2 magnetic nanosheets used in the present invention are prepared according to a method comprising the following steps: Sa, adding ammonia water into the dispersion of Fe3O4 magnetic nanosheets; Sb, adding the solution of butyl titanate dropwise to the solution obtained in step Sa to react; Sc. After dispersing the product obtained in step Sb, adding ammonia water, and then placing it in a reactor for heat treatment.
[0006] Specifically, in step Sa, a mixed solution of ethanol and acetonitrile is used to prepare the dispersion of the Fe3O4 magnetic nanosheets; In the dispersion, the mass-volume concentration of the Fe3O4 magnetic nanosheets is 0-2 mg / mL, preferably 1 mg / mL; The mass concentration of the ammonia water is 25-28%; The volume ratio of the ammonia water to the dispersion liquid is 0.25-1:100, preferably 0.5:100.
[0007] Specifically, in step Sb, a mixture of ethanol and acetonitrile is used to prepare the butyl titanate solution; Using a syringe to drop the solution of butyl titanate into the solution; The dosage of the butyl titanate is: 0.25-1.25 mL / 100 mg Fe3O4 magnetic nanosheets, preferably 0.75 mL / 100 mg Fe3O4 magnetic nanosheets.
[0008] The reaction temperature is room temperature and the reaction time is 1 to 4 hours.
[0009] Specifically, in step Sc, the product obtained in step Sb is dispersed in a mixed solution of ethanol and water, the aqueous ammonia is added under ultrasonic conditions, and the ultrasonic treatment is continued for 10 to 25 minutes before being transferred to the reactor.
[0010] Specifically, in step Sc, the heat treatment temperature is 120-180° C., and the time is 20-26 h.
[0011] Specifically, in step Sc, the Fe3O4-TiO2 magnetic nanosheets are separated from the heat-treated system by magnetic separation, and then washed several times with deionized water and anhydrous ethanol, and then placed in a freeze dryer for freeze drying.
[0012] Based on the Fe3O4-TiO2 magnetic nanosheets, the method for photocatalytically synergizing the Fenton-like reaction to catalyze and degrade dye wastewater provided by the present invention comprises the following steps: S1, adding Fe3O4-TiO2 magnetic nanosheets to the dye wastewater to be treated and protecting it from light; S2. Adding H2O2 to the dye wastewater to carry out a photocatalytic degradation reaction under light, thereby achieving catalytic degradation of the dye wastewater.
[0013] In the above method, in step S1, the dosage of the Fe3O4-TiO2 magnetic nanosheets is 1 g / L; The concentration of the dye in the dye wastewater is 10-50 mg / L, preferably 30 mg / L; The light-proofing treatment time is 20 to 60 minutes, preferably 30 minutes; The light-shielding treatment is performed under stirring conditions.
[0014] In the above method, in step S2, the amount of H2O2 added is 1~2mL, preferably 1.5mL.
[0015] The present invention not only provides a new research idea for the design and preparation of new catalytic degradation materials, but also provides a practical solution to the problem of wastewater treatment.
[0016] In the above method, the dyes in the dye wastewater are RhB, methylene blue (MB) and methyl orange (MO).
[0017] The Fe3O4-TiO2 magnetic nanosheets used in the method of the present invention have TiO2 and Fe3O4 tightly connected by chemical bonds, and the interface structure can induce the nanosheets to produce more active sites, thereby improving the catalytic performance thereof.
[0018] The Fe3O4-TiO2 magnetic nanosheets used in the method of the present invention introduce Fe3O4 into TiO2, and the existence of Ti-O-Fe bonds changes the transfer path of photogenerated carriers, thereby inhibiting the photogenerated e - -h + The catalytic activity of the catalyst is improved.
[0019] Under the action of an external magnetic field, the Fe3O4-TiO2 magnetic nanosheets used in the method of the present invention can be quickly separated from the dispersed solution, indicating that they have sufficient magnetism. The Fe3O4-TiO2 magnetic nanosheets of the present invention have good reusability.
[0020] The invention overcomes the limitations of traditional Fe3O4 nanoparticles by using Fe3O4-TiO2 magnetic nanosheets, and has the advantages of simple preparation, reusability, high catalytic degradation efficiency, etc. The unique two-dimensional nanostructure of Fe3O4-TiO2 magnetic nanosheets enables it to have better interaction with TiO2 nanoparticles, promoting the photogenerated electrons in TiO2 to effectively convert Fe3O4 nanoparticles into 3+ Reduction to Fe 2+ , inhibiting the recombination of photogenerated electron-hole pairs and improving the catalytic activity of the catalyst. Based on the good magnetic properties and high catalytic activity of Fe3O4-TiO2 magnetic nanosheets, it has excellent recyclability and stability. After 5 cycles, the photocatalytic degradation rate and recovery rate of the system of the present invention are still over 90%. The present invention achieves efficient, rapid and low-cost degradation of RhB dye wastewater, and provides a new research idea for the design and application of wastewater catalytic degradation materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 Schematic diagram of the synthesis of Fe3O4-TiO2 nanosheets according to the present invention.
[0022] Figure 2 Figure 2 is the N2 adsorption-desorption curve (Figure a) and pore size distribution curve (Figure b) of Fe3O4-TiO2 of the present invention.
[0023] Figure 3 XRD spectra of different samples.
[0024] Figure 4 This is the XPS spectrum of FT-0.75 (figures ad are survey, Fe 2p, Ti 2p and O 1 s respectively).
[0025] Figure 5 The SEM image of Fe3O4 (Figure a), the SEM image of FT-0.75 (Figure b), the TEM image of FT-0.75 (Figure c) and the HRTEM image of FT-0.75 (Figure d).
[0026] Figure 6 UV-vis spectrum (Figure a), Tauc plot (Figure b) and PL emission spectrum (Figure c) of the catalyst sample.
[0027] Figure 7 Figure 2 shows the degradation of RhB dye under different systems (Figure d) and the corresponding reaction rate constant k under different systems (Figure e).
[0028] Figure 8 The MH curves of Fe3O4 and FT-0.75 (Figure a, the upper left inset is the MH curve under low magnetic field, and the lower right inset is the magnetic separation photo), the cyclic experiment of FT-0.75+H2O2+light system to degrade RhB dye (Figure b), and the XRD spectrum of FT-0.75 before and after the cyclic experiment (Figure c). DETAILED DESCRIPTION
[0029] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0030] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0031] Example 1. Synthesis and Characterization of TiO2 Nanoparticles and Fe3O4-TiO2 Nanosheets 1. Synthesis Schematic Diagram Figure 1 shown.
[0032] Fe3O4 magnetic nanosheets (100 mg) were dispersed in 100 mL of anhydrous ethanol / acetonitrile mixed solution (3 / 1, v / v), and ultrasonicated to fully dissolve them. Then, NH3·H2O solution (0.50 mL) was added and ultrasonicated continuously. After fully dissolving, the solution was transferred to a three-necked flask and the stirring speed was set to 500 rpm. TBOT solution was added dropwise to 20 mL of anhydrous ethanol / acetonitrile mixed solution (3 / 1, v / v), magnetically stirred for 30 min, and then transferred to a 20 mL syringe. The syringe was installed on a syringe pump, and the syringe pump was set to add drops for 20 min. The solution was pushed dropwise into the three-necked flask. After the addition was completed, the reaction was continued for 2 h. After the reaction was completed, the product was separated and washed. The obtained product was then dispersed in anhydrous ethanol (40 mL) and deionized water (20 mL), and NH3·H2O solution (2.5 mL) was added under ultrasonic conditions. After ultrasonic treatment for 15 min, the mixture was transferred to a 100 mL reactor and heat treated at 160 ℃ for 24 h. After the high-pressure reactor was naturally cooled to room temperature, the product was separated by a magnet, and the obtained product was washed several times with deionized water and anhydrous ethanol, and the product was placed in a freeze dryer for freeze drying for 48 h.
[0033] The amount of TBOT solution added (TBOT dosage: 0.25, 0.5, 0.75, 1, 1.25 mL / 100 mg Fe3O4 magnetic nanosheets) was 0.25, 0.5, 0.75, 1, and 1.25 mL, respectively, and the corresponding nanosheets were labeled as FT-0.25, FT-0.5, FT-0.75, FT-1, and FT-1.25, respectively. If Fe3O4 nanoparticles are used, it is defined as SFT-0.75. The synthesized sample without Fe3O4 magnetic nanosheets is pure TiO2 nanoparticles.
[0034] 2. Structure and surface composition of Fe3O4 magnetic nanosheets Figure 2 N2 adsorption-desorption isotherms and BJH pore size distribution diagrams of Fe3O4-TiO2 nanosheets prepared with different TBOT dosages.
[0035] from Figure 2 As can be seen in Figure a, according to the IUPAC classification, the N2 adsorption-desorption isotherms of all catalyst samples are type IV, with an H3 hysteresis loop, which is a mesoporous structure. Figure 2 Figure b shows that there are a large number of mesopores with pore sizes ranging from 2 to 50 nm in the catalyst sample. More importantly, the specific surface area and pore volume of the catalyst sample increase first and then decrease with the increase of the TiO2 ratio. This may be due to the fact that a proper amount of TiO2 nanoparticles stack on the surface of the Fe3O4 magnetic nanosheets to form a large number of new mesopores, which increases the pore volume. However, when the TiO2 nanoparticles are excessive, some of the original pores will be masked, which will lead to a decrease in the pore volume. When the TBOT dosage is 0.75 mL, the specific surface area (121.67 m 2 ·g -1 ) and pore volume (0.554 cm 3 ·g -1 ) is the largest. The large specific surface area and rich pore structure are conducive to increasing its contact area with pollutants, thereby enhancing its adsorption and catalytic degradation performance of target pollutants. Therefore, FT-0.75 nanosheets are considered to be a good adsorption and photocatalytic material.
[0036] Figure 3 XRD spectra of TiO2 nanoparticles, Fe3O4 nanosheets and FT-0.75 nanosheets.
[0037] The XRD spectrum of TiO2 nanoparticles shows that the characteristic peaks at 2θ of 25.281°, 37.800°, 48.049°, 53.890°, 55.060°, 62.688°, 68.760°, 70.309° and 75.029° correspond to the (101), (004), (200), (105), (211), (204), (116), (220) and (215) crystal planes of anatase TiO2 (JCPDF No. 21-1272). Compared with rutile, anatase TiO2 is more conducive to the adsorption and photocatalytic oxidation of organic pollutants because it has a slower electron-hole pair recombination rate and a higher reduction potential. For Fe3O4 magnetic nanosheets, several characteristic peaks at 30.091°, 35.443°, 43.074°, 53.438°, 56.964° and 62.553° are consistent with the (220), (311), (400), (422), (511) and (440) crystal planes of cubic magnetite Fe3O4 (JCPDF 85-1436). These peaks are sharp and intense, and there are no other redundant peaks, which proves that the prepared samples are of high purity and good crystallinity. From the XRD spectrum of FT-0.75 nanosheets, it can be seen that in addition to the diffraction peaks caused by Fe3O4, there are also diffraction peaks of anatase TiO2, and after loading TiO2 nanoparticles, the diffraction peaks of Fe3O4 remain basically unchanged, indicating that the introduction of TiO2 nanoparticles has no effect on the crystal structure of Fe3O4 magnetic nanosheets.
[0038] In order to further verify the elemental composition and chemical state of the surface of FT-0.75 nanosheets, XPS tests were performed on FT-0.75 nanosheets. The results are as follows Figure 4 shown.
[0039] Figure 4 Figure a in the middle is the full spectrum of FT-0.75. It can be seen from the figure that Fe, Ti and O elements exist in FT-0.75. Figure 4 b shows the Fe 2p spectrum. 3 / 2 and Fe 2p 1 / 2 The binding energies of Fe 2+ (from FeO) and Fe 3+ (from Fe2O3) peak composition, indicating the presence of Fe3O4 in the nanosheets. Figure 4 Figure c shows the Ti 2p spectrum, where Ti 2p 3 / 2 and Ti 2p 1 / 2 There are two obvious peaks at 458.4 eV and 464.2 eV, respectively, which are consistent with the Ti 4+phase, indicating the formation of anatase TiO2. Figure 4 Figure d in the middle is the O 1s spectrum, and an obvious peak appears at 530.1 eV, which corresponds to the bond energy of the Ti-O-Fe bond. The existence of the Ti-O-Fe bond indicates that the combination of Fe3O4 and TiO2 is not a simple physical mixture, but is tightly bound by chemical bonds, which makes the FT-0.75 nanosheets have strong stability.
[0040] The morphology of the catalyst samples was characterized by scanning electron microscopy and transmission electron microscopy. Figure 5 shown.
[0041] like Figure 5 As shown in Figure a, the Fe3O4 catalyst sample is composed of polygonal nanosheets, and the majority of nanosheets are hexagonal. Figure 5 As can be seen in Figure b, TiO2 nanoparticles with a particle size of about 10-20 nm are uniformly deposited and loaded on the Fe3O4 magnetic nanosheets. Due to the deposition and coating of a large number of TiO2 nanoparticles on the Fe3O4 magnetic nanosheets, the FT-0.75 nanosheets present an irregular polygonal sheet structure. Figure 5 Figure c is a TEM image of FT-0.75 nanosheets, which further shows that FT-0.75 nanosheets are composed of Fe3O4 nanosheets and TiO2 nanoparticles. Figure 5 As shown in Figure d, the lattice spacing further confirms that the FT-0.75 nanosheets have two different crystal planes. Combined with the previous XRD analysis, the lattice spacing of 0.296 nm corresponds to the (220) plane of Fe3O4, and 0.3523 nm corresponds to the (101) plane of TiO2. In addition, it is worth noting that a connection is observed at the intersection of two different lattice spacings between Fe3O4 and TiO2, indicating that TiO2 nanoparticles are successfully deposited on the surface of Fe3O4 magnetic nanosheets. According to the previous XPS spectrum analysis, Ti-O-Fe bonds are formed at the intersection of Fe3O4 and TiO2, further indicating that TiO2 and Fe3O4 are tightly connected through chemical bonds, and the interface structure can induce FT-0.75 nanosheets to produce more active sites and improve their catalytic performance.
[0042] 3. Optical and photoelectrochemical properties of Fe3O4 magnetic nanosheets To study the light absorption capacity of the catalyst, the catalyst samples were subjected to UV-visible diffuse reflectance tests. Figure 6 shown.
[0043] like Figure 6As shown in Figure a, TiO2 has a strong light absorption edge in the ultraviolet region, and the absorption edge is located at 382 nm. The band gap width of Fe3O4 is 0.1 eV, which is a narrow-band semiconductor, so its light absorption capacity in the visible light region is more significant. After TiO2 nanoparticles are loaded onto the surface of Fe3O4 magnetic nanosheets, the absorption band edge of FT-0.75 nanosheets relative to TiO2 shows a significant red shift, proving that the introduction of narrow-bandgap semiconductors can effectively improve the visible light absorption capacity of photocatalysts. Figure 6 Figure b in the middle shows the energy gap of the catalyst sample, which is Figure 6 As shown in Figure b, the estimated band gaps of TiO2 and FT-0.75 are 3.25 eV and 1.65 eV, respectively, which can be attributed to the Fe 3+ (0.1064 nm) has an ionic radius close to that of Ti 4+ (0.1068 nm), during the recombination process, some Fe 3+ Can replace Ti 4+ The lattice position of TiO2 is changed to produce lattice defects, forming a new impurity band, which causes the valence band position of TiO2 to move up, while the conduction band position remains unchanged, the bandgap width becomes smaller, and the light response range is expanded.
[0044] In order to study the charge separation efficiency of the catalyst samples, the PL spectra of the catalyst samples were measured at an excitation wavelength of 385 nm, as shown in Figure 6 As shown in Figure c, TiO2 nanoparticles exhibit a higher PL intensity signal, indicating that electron-hole pairs are easy to recombine. The PL intensity signals of SFT-0.75 and FT-0.75 are relatively low, indicating that the introduction of Fe3O4 into the catalyst TiO2 enhances the photogenerated electrons. - -h + The separation ability of the pairs makes it less likely to recombine. In contrast, the PL intensity signal of FT-0.75 is the lowest. This can be attributed to the fact that the Fe3O4 magnetic nanosheets are controlled by a specific crystal plane, and the unique surface structure makes it have a large contact area with the TiO2 nanoparticles, thus promoting the photogenerated - Transfer from TiO2 nanoparticles to Fe3O4 magnetic nanosheets, photogenerated - -h + The separation efficiency is higher and the photocatalytic activity is higher. In addition, after the introduction of Fe3O4 into the catalyst TiO2, the presence of Ti-O-Fe bonds changes the transfer path of photogenerated carriers and inhibits the photogenerated e - -h + The catalytic activity of the catalyst is improved.
[0045] Example 2: Degradation of RhB dye wastewater by FT-0.75 photocatalytic synergistic Fenton-like reaction 1. Photocatalytic synergistic Fenton-like reaction experiment The UV analyzer was selected as the light source and the RhB dye solution was selected as the target pollutant. The catalytic degradation effect of Fe3O4-TiO2 nanosheets was evaluated by measuring the decolorization of the RhB dye solution under light irradiation.
[0046] Specific catalytic degradation experimental steps: Weigh a certain amount of Fe3O4-TiO2 nanosheets as catalyst and place them in 100mL, 30mg·L -1 The RhB dye solution was stirred and protected from light for 30 min to allow the Fe3O4-TiO2 nanosheets to reach adsorption-desorption equilibrium with the dye. The supernatant was separated by magnet, and the absorbance of the RhB dye solution was detected at a peak absorption wavelength of 553 nm using a UV-visible spectrophotometer. Then a certain amount of H2O2 was added, and the light source was turned on to start the photocatalytic degradation reaction. Every 20 min, the supernatant was separated by magnet, the absorbance was detected, and converted into concentration according to the Lambert-Beer law, and its degradation rate was calculated.
[0047] The calculation method of RhB dye solution degradation rate is shown in formula (1): (1) Where C0 is the initial concentration of the RhB dye solution after the dark reaction is completed and before illumination, in mg·L -1 ; C is the concentration of RhB dye solution at time t of illumination, in mg·L -1 .
[0048] 2. Photocatalytic degradation performance of FT-0.75 in synergistic Fenton-like reaction Firstly, the effect of Fe3O4-TiO2 nanosheets prepared at different TBOT dosages on the catalytic degradation of RhB dye solution was investigated. Figure 7 shown.
[0049] The results show that with the increase of TBOT dosage, the degradation behavior of the Fe3O4-TiO2 nanosheets of the present invention on RhB dye shows a trend of first increasing and then decreasing. The degradation efficiency of the FT-0.75 nanosheet is the highest, reaching 98.12%. This can be attributed to the higher specific surface area of FT-0.75 and the effective separation of electron-hole pairs. At the same time, under the action of the FT-0.75 nanosheet, the changes in the absorption spectrum of the RhB dye solution exposed to light at different time intervals and the corresponding photo records show that the main absorption peak of RhB at 553nm decreases with the increase of irradiation time, and the color of the RhB dye solution gradually becomes lighter until it is close to transparent, indicating that the RhB dye is removed. The FT-0.75 nanosheet shows a higher degradation efficiency.
[0050] In order to further illustrate the effectiveness of the FT-0.75 photocatalytic synergistic Fenton-like system, the present invention conducted a series of experiments to study the degradation of RhB dye by different reaction systems. Figure 7 As shown in Figure d, when light is used alone, the concentration of RhB dye remains almost unchanged and the self-photolysis effect can be ignored. For the H2O2+light system, since light irradiation can promote the decomposition of H2O2 to produce active substances ·OH, the degradation rate can reach 43.12%. After adding photocatalysts TiO2 and FT-0.75 under light conditions, a photocatalytic oxidation reaction occurs, and the degradation rate is further improved. In addition, the degradation rate of the photocatalytic system with FT-0.75 as the catalyst (65.91%) is higher than the degradation rate of the photocatalytic system with TiO2 as the catalyst (51.01%). This is mainly because the Fe in the Fe3O4 magnetic nanosheets 3+ It captures the photogenerated - Fe 2+ , inhibiting the photogenerated - -h + The composite improves the photocatalytic performance. For the heterogeneous photo-Fenton system (Fe3O4+H2O2+light), the degradation rate of RhB dye can reach 76.36%. For the photocatalytic synergistic Fenton system (FT-0.75+H2O2+light), the degradation rate of RhB dye is further improved to 98.12%. This may be due to the unique two-dimensional nanostructure of Fe3O4 magnetic nanosheets, which is conducive to its good interaction with TiO2 nanoparticles. The photogenerated electrons generated by TiO2 under light interact with Fe 3+ The reaction generates Fe 2+ , which promotes Fe 3+ / Fe 2+ The cycle of photocatalytic reaction increases the rate of Fenton-like reaction. At the same time, the recombination of photogenerated electron-hole pairs is also suppressed during the photocatalytic reaction, further increasing the reaction rate.
[0051] In order to make a more comprehensive comparison, the catalytic degradation data of RhB dye were further analyzed using the fitted first-order kinetic equation: (2) Among them, C (mg·L -1 )、C0(mg·L -1 )、t(min)、k(min -1 ) are respectively the concentration of RhB dye after irradiation, the initial concentration of RhB dye, the irradiation time, and the reaction rate constant. Figure 7 As shown in Figure e, the k value of FT-0.75+H2O2+light (0.03301 min -1) are FT-0.75+light (0.008680 min -1 ) and Fe3O4+H2O2+light(0.01209min -1 ), which further illustrates that in the FT-0.75+H2O2+light system, photocatalysis and Fenton-like reaction have a synergistic effect, further improving the reaction rate.
[0052] 3. Reusability and stability of FT-0.75 nanosheets The reusability and stability of catalysts are important factors affecting their practical applications. Figure 8 Figure a shows the hysteresis loop of the catalyst sample measured by VSM. The residual magnetization of FT-0.75 nanosheets (3.27 emu g -1 ) and coercivity (58.4 Oe) are negligible, indicating that it has typical superparamagnetism. The saturation magnetization of Fe3O4 nanosheets is 68.3 emu g -1 After the deposition of TiO2 nanoparticles, the magnetic properties of FT-0.75 nanosheets decreased, and the saturation magnetization was 34.5 emu·g -1 Nevertheless, under the action of an external magnetic field, FT-0.75 nanosheets can be quickly separated from the dispersed solution, indicating that they have sufficient magnetic properties.
[0053] The reusability of FT-0.75 nanosheets in a photocatalytic synergistic Fenton-like system was evaluated by a RhB dye degradation cycle experiment. After each cycle, the catalyst was separated from the solution by a magnet, washed, dried, and used in the next cycle while keeping other reaction conditions unchanged. Figure 8 As shown in Figure b, as the number of cycles increases, the recovery rate of FT-0.75 nanosheets decreases, which may be due to the loss of catalyst during the cleaning process. In addition, the catalytic degradation rate of RhB dye by FT-0.75 nanosheets decreases. This may be because after the cycle, the pollutants are adsorbed on the catalyst surface, the active sites are reduced, and thus the degradation efficiency of RhB dye is affected. However, after 5 cycles, the recovery rate of FT-0.75 nanosheets and the degradation rate of RhB dye can still exceed 90%, indicating that FT-0.75 nanosheets have good reusability.
[0054] In addition, the excellent stability of FT-0.75 nanosheets can also be observed from the fresh and used XRD patterns (e.g. Figure 8As shown in Figure c), there is no significant difference in the crystal structure of the FT-0.75 nanosheets before and after 5 cycles. Therefore, the FT-0.75 nanosheets used in the method of the present invention can be used as an efficient and recyclable catalyst for wastewater treatment of organic pollutants.
Claims
1. A method for photocatalytic degradation of dye wastewater by Fenton-like reaction, comprising the following steps: S1, adding Fe3O4-TiO2 magnetic nanosheets to the dye wastewater to be treated and protecting it from light; S2, adding H2O2 to the dye wastewater, and performing a photocatalytic degradation reaction under light, that is, achieving catalytic degradation of the dye wastewater; The Fe3O4-TiO2 magnetic nanosheets are prepared according to a method comprising the following steps: Sa, adding ammonia water into the dispersion of Fe3O4 magnetic nanosheets; Sb, adding the solution of butyl titanate dropwise to the solution obtained in step Sa to react; Sc. After dispersing the product obtained in step Sb, adding ammonia water, and then placing it in a reactor for heat treatment.
2. The method according to claim 1, characterized in that: In step S1, the dosage of the Fe3O4-TiO2 magnetic nanosheets is 1 g / L; the concentration of the dye in the dye wastewater is 10-50 mg / L; The light-proofing treatment time is 20 to 60 minutes; The light-shielding treatment is performed under stirring conditions.
3. The method according to claim 1 or 2, characterized in that: In step S2, the amount of H2O2 added is 1 to 2 mL.
4. The method according to any one of claims 1 to 3, characterized in that: The dyes in the dye wastewater are rhodamine B, methylene blue and methyl orange.
5. The method according to any one of claims 1 to 4, characterized in that: In step Sa, a dispersion of the Fe3O4 magnetic nanosheets is prepared using a mixed solution of ethanol and acetonitrile; In the dispersion, the mass-volume concentration of the Fe3O4 magnetic nanosheets is 0 to 2 mg / mL; The mass concentration of the ammonia water is 25-28%; The volume ratio of the ammonia water to the dispersion liquid is 0.25 to 1:
100.
6. The method according to any one of claims 1 to 5, characterized in that: In step Sb, a mixture of ethanol and acetonitrile is used to prepare the butyl titanate solution; Using a syringe to drop the solution of butyl titanate into the solution; The dosage of the butyl titanate is: 0.25-1.25 mL / 100 mg Fe3O4 magnetic nanosheets; The reaction temperature is room temperature and the reaction time is 1 to 4 hours.
7. The method according to any one of claims 1 to 6, characterized in that: In step Sc, the product obtained in step Sb is dispersed in a mixed solution of ethanol and water, and the aqueous ammonia is added under ultrasonic conditions, and the ultrasonic treatment is continued for 10 to 25 minutes before being transferred to the reactor.
8. The method according to any one of claims 1 to 7, characterized in that: In step Sc, the heat treatment temperature is 120-180° C. and the time is 20-26 hours.
9. The method according to any one of claims 1 to 8, characterized in that: In step Sc, the Fe3O4-TiO2 magnetic nanosheets are separated from the heat-treated system by magnetic separation.
Citation Information
Patent Citations
Dielectric barrier discharge plasma-fenton-like-photocatalysis method for degrading organic matter
CN104058481A
Photo-Fenton catalyst Fe3O4 / rGO / TiO2, preparation method and applications thereof
CN106238053A
Wastewater treatment method with low sludge yield based on multi-dimensional catalytic oxidation process
CN113135631A
Paste for manufacturing photocatalyst and manufacturing method of photocatalyst
US20170304806A1
A fe 3o 4@d-wood photocatalyst
WO2024104637A1
Cited By
Preparation of solar photo-thermal conversion material with strong near-infrared light absorption and application of solar photo-thermal conversion material in degradation of organic pollutants
CN119349693A
Preparation of solar thermal conversion materials with strong near-infrared light absorption and their application in degradation of organic pollutants
CN119349693B