Preparation method and application of FeMo-BC

Through the joint conditioning method of FeMo-BC composite materials, the sludge floc structure is broken and the porosity is increased, which solves the problem of difficulty in deep dewatering of sludge and achieves efficient dehydration of sludge and cost reduction.

CN118754391APending Publication Date: 2024-10-11YANGTZE ECOLOGY & ENVIRONMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410787203.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing technology has problems such as insufficient destruction of the EPS network structure, increased sludge viscosity, and blockage of water passages during the deep dehydration process of sludge, which makes deep dehydration of sludge difficult and lacks a highly active persulfate activator.

Method used

FeMo-BC composite material is prepared through potassium ferrate activation method and hydrothermal method, combined with PMS and TA for joint conditioning, breaking the sludge floc structure, releasing bound water, and through the skeleton support and electrical neutralization of FeMo-BC Improve the porosity and permeability of sludge.

Benefits of technology

Significantly reduce the compressibility and water content of sludge, improve the dehydration effect of sludge, and reduce post-processing costs. Optimizing the optimal concentration of FeMo-BC and the PMS/TA ratio can significantly reduce the SRF and mud cake of sludge. Moisture content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754391A_ABST
    Figure CN118754391A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of FeMo-BC. The preparation method comprises the following steps: by taking waste biomass bamboo powder as a raw material, activating with potassium ferrate, and then mixing with molybdate and a sulfur-containing reducing agent to prepare FeMo-BC through two steps of a hydrothermal method; according to the application, FeMo-BC, PMS and TA are used for constructing a combined conditioning system for sludge conditioning, on one hand, a floc structure of PMS oxidized and crushed sludge can be efficiently activated, and release of bound water is promoted; on the other hand, the metal-loaded carbon-rich particles can play roles of electric neutralization, adsorption and skeleton support. In the sludge conditioning process, protein and fine floc particles in the sludge are further flocculated and precipitated in combination with TA, an oxidation-skeleton support-re-flocculation combined conditioning method is constructed, deep dehydration of the sludge can be promoted, and the post-treatment cost of the sludge is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of sludge conditioning and dehydration, and particularly relates to a preparation method and application of FeMo-BC. Background Art

[0002] The water content of municipal sludge can generally reach 95%-99.5%, and it is rich in organic matter, of which extracellular polymers (EPS) account for more than half of the total organic matter. At present, the high water content of municipal sludge has greatly restricted the reduction and resource utilization of sludge, and it is urgent to develop new technologies for deep sludge dehydration.

[0003] Studies have shown that EPS in sludge exists in the center or surface of sludge flocs in a network structure, which limits the removal of water during the filter press process. Breaking down EPS can effectively improve the sludge dewatering performance. The Fenton process can produce strong oxidizing free radicals, which are usually used to remove organic pollutants in sewage. Its extended persulfate oxidation method can generate sulfate free radicals (SO4 - ·), has the advantages of strong oxidizability and little influence by pH value, and has received more extensive attention. The method of activating peroxymonosulfate includes thermal activation, micro-wave activation, ultrasonic activation, alkali activation, transition metal activation, etc., among which transition metal iron has received extensive attention because of its low price and pollution-free. For example, CN117654625B discloses a natural polysaccharide modified biological iron-based catalytic material and its preparation method and application, which utilizes a culture medium containing an iron source to cultivate iron-mineralized bacteria to obtain iron-mineralized bacteria cells and cell suspensions thereof, and then cultivates the cell suspension, filters it by suction, washes and freeze-dries it to obtain a natural polysaccharide modified biological iron-based catalytic material, which can be used as a Fenton-like catalyst, with hydrogen peroxide or peroxymonosulfate as an oxidant, to achieve the degradation of organic pollutants.

[0004] After activation, persulfate can effectively destroy sludge flocs and sludge microbial cells, release intracellular bound water, and improve sludge dewatering performance. Therefore, it has a high research value in sludge conditioning. 2+ Activated PDS conditioning sludge dewatering, at 1.2 mmol∙g −1 VSS PDS, 1.5 mmol∙g −1 VSS Fe 2+ , pH 3.00-8.50, CST can be reduced by 88.80% within 1 min. Ding Jinglin used biomass and potassium ferrate co-pyrolysis to prepare biochar loaded with nano-zero-valent iron to activate persulfate to remove estradiol (E2), and found that its removal effect on E2 was significantly better than that of biochar and nano-zero-valent iron alone.

[0005] However, the single use of oxidation to destroy EPS in sludge can easily cause the sludge viscosity to increase, and the tiny flocs formed by the broken EPS network structure will block the water passage in the sludge, making it difficult to dehydrate the sludge deeply. Therefore, how to increase the supporting role in the sludge filter press dewatering process to reduce the compressibility of the mud cake and improve the porosity and permeability of the sludge is an urgent problem to be solved in the process of using peroxymonosulfate to condition the sludge; in addition, it is also necessary to continue to develop highly active peroxymonosulfate activators. Summary of the invention

[0006] In view of the above technical problems, the present invention provides a preparation method and application of FeMo-BC. FeMo-BC is prepared in two steps using waste biomass bamboo powder as raw material by potassium ferrate activation method and hydrothermal method. It is used for sludge conditioning. On the one hand, it can efficiently activate the floc structure of PMS oxidation-broken sludge and promote the release of bound water; on the other hand, the metal-loaded carbon-rich particles can play the role of electrical neutralization, adsorption and skeleton support. In the process of sludge conditioning, TA flocculation is further combined to precipitate proteins and fine floc particles in the sludge, and an oxidation-skeleton support-reflocculation combined conditioning method is constructed, which can promote the deep dehydration of sludge and reduce the post-processing cost of sludge.

[0007] In order to achieve the above object, the present invention provides an application of FeMo-BC, wherein the application is application in sludge conditioning.

[0008] Preferably, the sludge conditioning is to reduce the water content and / or sludge specific resistance of the sludge.

[0009] Further preferably, the conditioning of the water content of the sludge includes reducing CST and / or mud cake Wc and degrading flocculated EPS.

[0010] Preferably, the application is to condition sludge by combining FeMo-BC, PMS and TA.

[0011] Further preferably, the mass ratio of FeMo-BC, PMS and TA is 8-15:2-6:2-6.

[0012] More preferably, the mass ratio of FeMo-BC, PMS and TA is 10:4:4.

[0013] Further preferably, the total amount of FeMo-BC, PMS and TA used in the combined sludge conditioning is 1.0%-2.5% of the dry weight of the sludge.

[0014] More preferably, the total amount of FeMo-BC, PMS and TA is 1.8% of the sludge mass.

[0015] Further preferably, the combined conditioning time is 20-50 min, and the sludge pH value during the combined conditioning is 2-6.

[0016] Further preferably, the combined conditioning time is 30 minutes, and the sludge pH value during the combined conditioning is 4.

[0017] The present invention also provides a method for preparing FeMo-BC, comprising the following steps: (1) Dissolving biomass powder and ferrate in water, stirring evenly, drying, and pyrolyzing under an inert atmosphere to obtain Fe-BC; (2) Fe-BC is mixed with molybdate, a sulfur-containing reducing agent and water, and after hydrothermal reaction, the mixture is centrifuged, washed and dried to obtain FeMo-BC.

[0018] Preferably, the mass ratio of the biomass powder to ferrate in step (1) is 1.5:4.

[0019] Further preferably, the biomass powder is bamboo powder, and the ferrate is potassium ferrate.

[0020] Preferably, the pyrolysis temperature in step (1) is 450-650°C.

[0021] Preferably, the mass ratio of Fe-BC to molybdate in step (2) is 1-2:1-3.

[0022] Preferably, the mass ratio of the molybdate to the sulfur-containing reducing agent in step (2) is 1:2.

[0023] Further preferably, the molybdate is sodium molybdate, and the sulfur-containing reducing agent is thiourea.

[0024] Preferably, the hydrothermal reaction conditions in step (2) are 160-200° C. for 8-14 h.

[0025] The beneficial effects of the present invention are: 1. Abandoned bamboo chopsticks were ground into biomass powder, and then FeMo-BC composite materials that can efficiently activate PMS were prepared by ferrate activation method and hydrothermal method, which reduced the raw material cost, enriched the types of Fenton-like system catalysts, and improved the activation efficiency of PMS.

[0026] 2. A FeMo-BC / PMS / TA combined conditioning system was established to jointly condition municipal sludge, which caused the sludge floc structure to break up, forming cracks and holes. The free radical oxidation made the sludge particle size smaller, releasing the bound water inside the sludge flocs. At the same time, FeMo-BC can also be used as a skeleton material to construct a dehydration channel, providing a channel for the escape of water. Through the complexation and precipitation of TA, the protein and polysaccharide content of EPS was significantly reduced, and the broken sludge particles and the oxidized and shrunk sludge flocs were re-flocculated and precipitated, reducing the compressibility of the mud cake and improving the dehydration effect of the sludge.

[0027] 3. The optimal concentration of FeMo-BC in the FeMo-BC / PMS / TA combined conditioning system is 100 mg / g, and the optimal concentrations of PMS and TA are both 40 mg / g. At a pH of 4, the sludge SRF and mud cake CST can be significantly reduced, and the EPS content can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the effect of FeMo-BC prepared at different pyrolysis activation temperatures on sludge conditioning in Example 2.

[0029] Figure 2 FeMo-BC prepared at different Mo contents in Example 3 and the effect of Fe-BC on sludge conditioning.

[0030] Figure 3 These are SEM images of BC, Fe-BC and FeMo-BC in Example 5, where a is BC, b is Fe-BC, and c is FeMo-BC.

[0031] Figure 4 These are the EDS images of the elements in FeMo-BC in Example 5, where a is the SEM image of the FeMo-BC micro-area, b is the distribution map of the oxygen element in FeMo-BC, c is the distribution map of the iron element in FeMo-BC, d is the distribution map of the carbon element in FeMo-BC, e is the distribution map of the molybdenum element in FeMo-BC, and f is the distribution map of the sulfur element in FeMo-BC.

[0032] Figure 5 This is the XRD diagram of Fe-BC and FeMo-BC in Example 5.

[0033] Figure 6 This is the effect of the FeMo-BC concentration on sludge conditioning in Example 6.

[0034] Figure 7 This is the effect of the PMS concentration on sludge conditioning in Example 7.

[0035] Figure 8This is the effect of TA usage concentration on sludge conditioning in Example 8.

[0036] Fig. 9 This is the effect of sludge pH on sludge conditioning in Example 9.

[0037] Fig.10 This is the effect of conditioning time on sludge conditioning in Example 10.

[0038] Fig.11 This is the effect of different conditioning systems on sludge conditioning in Example 11.

[0039] Fig.12 This is the effect of different conditioning methods on EPS in Example 12, where a is the protein in EPS and b is the polysaccharide in EPS.

[0040] Fig.13 These are SEM images of the sludge before and after conditioning in Example 13, where a is the sludge before conditioning and b is the sludge after conditioning.

[0041] Fig.14 This is the XRD diffraction pattern of the sludge cake before and after conditioning in Example 13. DETAILED DESCRIPTION

[0042] The technical solution of the present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It is worth noting that the following embodiments are only preferred embodiments of the present invention and should not be understood as limiting the present invention. The protection scope of the present invention shall be based on the contents recorded in the claims. Any modification or replacement made by those skilled in the art to the technical solution of the present invention without creative work shall fall within the protection scope of the present invention.

[0043] In the following examples, the sludge was taken from the Hewenhu Phase II Sewage Treatment Plant of Jiangxi Jiujiang Three Gorges Water Co., Ltd. The initial pH value of the sludge was 6.9, the water content was 98.8%, the capillary absorption time was 29.3s, and the sludge specific resistance was 9.77×10 11 m / kg, and the moisture content of the filter cake was 85.68%.

[0044] Example 1 Preparation of FeMo-BC (1) crushing discarded bamboo chopsticks and passing through a 200-mesh sieve to obtain bamboo powder; (2) immersing bamboo powder and potassium ferrate in deionized water, stirring them evenly, and then drying them at 60° C. to obtain a mixture, wherein the mass ratio of bamboo powder, potassium ferrate and deionized water is 1.5:4:50; (3) The mixture was transferred to a tube furnace and pyrolyzed at 350°C, 450°C, 550°C, 650°C and 750°C in a nitrogen atmosphere to prepare Fe-BC; (4) Place Fe-BC, sodium molybdate and thiourea in deionized water and stir to obtain a mixed solution, wherein the mass ratio of Fe-BC, sodium molybdate and thiourea is 1:1:2, and the total mass of the three substances is 4% of the deionized water; (5) The mixed solution was transferred to a reactor and subjected to hydrothermal reaction at 180 °C for 10 h. The precipitate was then retained by centrifugation, washed three times with deionized water, and dried at 60 °C to obtain FeMo-BC.

[0045] Example 2 Sludge Conditioning (1) At room temperature, stir the sludge thoroughly and adjust the pH value to 4; (2) FeMo-BC prepared at different pyrolysis temperatures in Example 1 was added to the sludge, and PMS and TA were added, and the mixture was stirred at 120 r / min for 30 min to complete the conditioning, wherein the concentration of FeMo-BC was 100 mg / g, and the concentrations of PMS and TA were both 40 mg / g; (3) After conditioning, the sludge specific resistance (SRF) is measured using a sludge specific resistance meter, and then filter press is performed to obtain a filter cake. The filter cake is dried at 105°C to a constant weight, the weight difference is measured, and the moisture content (Wc) of the filter cake is calculated.

[0046] The results are as follows Figure 1 As shown in the figure, as the pyrolysis temperature increases from 350℃ to 550℃, the SRF of the sludge increases from 4.52×10 11 m / kg decreased to 2.59×10 11 m / kg, and the mud cake Wc decreased from 77.2% to 70.64%. This is because as the temperature increases, potassium ferrate as an activator is more likely to diffuse on the surface of biochar, and the etching effect on the carbon pore wall is enhanced, which increases the porosity of biochar, is beneficial to the loading of metal particles, and improves the effect of catalyst activation of PMS. However, with the further increase of pyrolysis activation temperature, the pore destruction rate of bamboo-based biochar increases, even exceeding the pore generation rate, and the overall structure of biochar is more susceptible to ablation. Moreover, at higher temperatures, the valence state of iron will gradually change, which will eventually affect the activation effect of FeMo-BC on PMS and reduce the sludge dehydration effect. Therefore, 550℃ was selected as the optimal pyrolysis temperature.

[0047] Comparative Example 1 Preparation of Fe-BC (1) crushing discarded bamboo chopsticks and passing through a 200-mesh sieve to obtain bamboo powder; (2) immersing bamboo powder and potassium ferrate in deionized water, stirring them evenly, and then drying them at 60° C. to obtain a mixture, wherein the mass ratio of bamboo powder, potassium ferrate and deionized water is 1.5:4:50; (3) The mixture was transferred to a tube furnace and pyrolyzed at 550 °C in a nitrogen atmosphere to prepare Fe-BC.

[0048] Comparative Example 2 (1) crushing discarded bamboo chopsticks and passing through a 200-mesh sieve to obtain bamboo powder; (2) immersing bamboo powder in deionized water, stirring evenly, and then drying at 60° C. to obtain a mixture, wherein the mass ratio of bamboo powder, potassium ferrate and deionized water is 1.5:4:50; (3) The mixture was transferred to a tube furnace and pyrolyzed at 550 °C in a nitrogen atmosphere to prepare BC.

[0049] Example 3 Effect of Mo content on sludge dewatering (1) The method and steps are the same as those in Example 1, wherein the pyrolysis temperature in step (3) is 550° C., and the mass ratio of Fe-BC to sodium molybdate in step (4) is changed to 2:1, 1:1, 2:3, and 1:2, respectively, to adjust the Mo content in FeMo-BC; and then the sludge is conditioned according to the method and steps described in Example 2; (2) Then, Fe-BC was prepared in Comparative Example 1, and sludge was conditioned according to the method and steps described in Example 2; (3) Determination of the sludge specific resistance (SRF) of the conditioned sludge and the moisture content (Wc) of the filter cake The results are as follows Figure 2 As shown in the figure, when the ratio of Fe-BC to sodium molybdate increased from 2:1 to 1:1, the sludge SRF increased from 5.05×10 11 m / kg decreased to 2.59×10 11 m / kg, the mud cake Wc decreased from 77.93% to 70.64%, and the sludge dewatering effect was improved, which was better than the effect of using Fe-BC alone. This is because the surface of Fe-BC is loaded with a proper amount of MoS2 particles, and Fe 2+ / Fe 3+ and Mo 4+ / Mo 6+ The cycle of Mo 4+ The presence of Fe 3+ Fe 2+ Conversion, thus quickly activating PMS to produce a large amount of SO4 - · and other active free radicals, thereby accelerating the destruction of sludge EPS and converting intracellular bound water into free water. However, as the dosage of sodium molybdate gradually increased, the sludge SRF increased to 6.84×10 11m / kg, and the mud cake Wc also increased to 80.24%. It is speculated that too many MoS2 particles attached to the biochar surface, affecting the synergistic reaction between MoS2 and the iron oxides loaded on the biochar surface, resulting in a decrease in the catalytic activity of FeMo-BC and a decrease in the sludge dewatering performance. Therefore, the optimal mass ratio of Fe-BC to sodium molybdate is 1:1.

[0050] Example 4 The method and steps are the same as those in Example 1, wherein the pyrolysis temperature in step (3) is 550°C to prepare FeMo-BC.

[0051] Example 5 The Fe-BC prepared in Comparative Example 1, the BC prepared in Comparative Example 2, and the FeMo-BC prepared in Example 4 were analyzed by SEM, EDS and XRD.

[0052] SEM results are as follows Figure 3 As shown, the surface of BC is smooth and closed with few pores ( Figure 3 a); After being modified by potassium ferrate, Fe-BC is formed, and many small particles appear on the surface ( Figure 3 b) These evenly distributed iron oxides increase the active sites on the biochar surface and enhance the activation of PMS. At the same time, the introduction of iron oxide can improve the mechanical strength of the skeleton material. After loading MoS2 through hydrothermal reaction, a layer of MoS2 is evenly distributed on the surface of the biochar, and the MoS2 particles are distributed on the surface of the biochar in a flower-like manner ( Figure 3 c), and the iron-containing particles can limit the agglomeration of MoS2 particles. At the same time, the biochar treated by the hydrothermal process becomes more fluffy and can be used as a skeleton material to construct a dehydration channel during the sludge dehydration process, which is beneficial to the removal of water from the sludge flocs.

[0053] EDS results show that FeMo-BC contains Fe, O, C, Mo, and S elements, and the distribution areas of Fe and O elements are highly overlapped ( Figure 4 ), which confirmed the presence of iron-containing oxides on the surface of FeMo-BC, indicating that potassium ferrate successfully modified bamboo powder. In addition, the distribution of Mo and S elements is basically the same, which can confirm that MoS2 is successfully synthesized on the surface of biochar. In summary, it can be concluded that FeMo-BC composite materials were successfully prepared by potassium ferrate activation and hydrothermal synthesis.

[0054] From the XRD spectrum, we can find that ( Figure 5), Fe-BC has characteristic peaks at 30.1°, 35.4°, 43.1°, 56.9° and 62.5°, which correspond to the diffraction peaks of the (220), (311), (400), (511), and (440) crystal planes of Fe3O4 (JCPDS 99-0073), while the XRD spectrum of FeMo-BC is basically consistent with the characteristic peaks appearing in the XRD spectrum of Fe-BC, and the intensity is higher than the characteristic peaks of Fe-BC. The diffraction peak of MoS2 loaded in FeMo-BC is not obvious, and its phase was not found after analysis using MDI Jade 6 software, which is due to the low crystallinity of MoS2 on the surface of Fe-BC.

[0055] Example 6 Effect of FeMo-BC concentration on sludge dewatering (1) At room temperature, stir the sludge evenly, adjust the pH value to 4, and then divide it evenly into 5 groups; (2) FeMo-BC was added to each group of sludge to a concentration of 50 mg / g, 100 mg / g, 150 mg / g, 200 mg / g and 250 mg / g, and PMC and TA were added at the same time to a concentration of 40 mg / g; (3) After the addition is completed, stir the reaction at 120r / min for 30 minutes to complete the conditioning; (4) After conditioning, the sludge specific resistance (SRF) is measured using a sludge specific resistance meter, and then filter press is performed to obtain a filter cake. The filter cake is dried at 105°C to a constant weight, the weight difference is measured, and the moisture content (Wc) of the filter cake is calculated.

[0056] The results are as follows Figure 6 As shown in the figure, when the concentration of FeMo-BC is lower than 100 mg / g during conditioning, SRF and Wc both decrease with the increase of FeMo-BC. On the one hand, more FeMo-BC can increase the active sites that can participate in the reaction, so that PMS can be fully activated, more active free radicals are generated, and the removal rate of sludge EPS is increased. On the other hand, FeMo-BC plays a skeleton role for sludge to pass through more water channels. At the same time, FeMo-BC can also use the hydrophobic effect of the biochar surface to adsorb sticky substances in the sludge structure, thereby improving the dewatering performance of sludge. When the concentration of FeMo-BC after addition is greater than 150 mg / g, SRF and Wc increase significantly, indicating that too much FeMo-BC is not conducive to sludge dewatering. This is because too much FeMo-BC causes PMS to be consumed too quickly and cannot effectively break up sludge flocs. In addition, adding too much solid matter will also increase the total amount of dry sludge, weakening the advantage of sludge dewatering. Therefore, the optimal concentration of FeMo-BC in this conditioning system is 100 mg / g.

[0057] Example 7 Effect of PMC concentration on sludge dewatering The method and steps are the same as those in Example 6, except that the concentration of FeMo-BC in step (2) is controlled at 100 mg / g, and the dosage of PMC is adjusted to have concentrations of 20 mg / g, 30 mg / g, 40 mg / g, 50 mg / g and 60 mg / g, respectively, to complete the conditioning and detect the corresponding indicators.

[0058] The results are as follows Figure 7 As shown in the figure, as the concentration of PMS increases from 20 mg / g to 60 mg / g, the sludge SRF and mud cake Wc both show a trend of first decreasing and then increasing. When the concentration of PMS increases from 20 mg / g to 40 mg / g, the sludge dehydration effect is the best. This is because when the concentration of PMS increases, more SO4 can be produced in the system. - Participate in the oxidation and decomposition of sludge EPS, fully release the bound water in EPS, and improve the sludge dewatering performance. However, when the PMS concentration is too high, the sludge SRF and mud cake Wc will increase instead. The reason is that excessive PMS in the system will cause PMS to produce self-quenching reaction, and excessive HSO5 - With SO4 - Will produce SO5 - ·, seriously hindering the activation reaction of persulfate and reducing the overall sludge dewatering efficiency.

[0059] Example 8 Effect of TA concentration on sludge dewatering The method and steps are the same as those of Example 6. The concentration of FeMo-BC in step (2) is controlled at 100 mg / g, and the dosage of TA is adjusted to have a concentration of 20 mg / g, 30 mg / g, 40 mg / g, 50 mg / g and 60 mg / g, respectively. The conditioning is completed and the corresponding indicators are tested.

[0060] The results are as follows Figure 8 As shown in the figure, when the concentration of TA increased from 20 mg / g to 40 mg / g, the sludge SRF increased from 3.02×10 11 m / kg decreased to 2.59×10 11 m / kg, the CST of the sludge dropped to 17 s. This is because the increase in TA concentration accelerated the conversion rate of the iron-molybdenum valence state in the reaction system, increased the concentration of free radicals in the system, and TA had a complexing effect on the sludge flocs, which could promote the polymerization of small sludge flocs after the release of bound water to produce large flocs, which was beneficial to the sludge dewatering. However, when the concentration continued to increase, the sludge SRF would gradually increase. This was because excessive TA would quench the free radicals generated by the system, reduce the free radicals participating in the reaction, and weaken the degree of destruction of the sludge EPS. Therefore, this experiment determined that the optimal concentration of TA was 40 mg / g.

[0061] Example 9 Effect of sludge pH on sludge dewatering (1) At room temperature, the sludge was fully stirred and divided into 5 groups, and the pH values ​​were adjusted to 2, 3, 4, 5 and 6 respectively using 1 mol / L hydrochloric acid solution; (2) FeMo-BC prepared at different pyrolysis temperatures in Example 1 was added to the sludge, and PMS and TA were added, and the mixture was stirred at 120 r / min for 30 min to complete the conditioning, wherein the concentration of FeMo-BC was 100 mg / g, and the concentrations of PMS and TA were both 40 mg / g; (3) After conditioning, the sludge specific resistance (SRF) is measured using a sludge specific resistance meter, and then filter press is performed to obtain a filter cake. The filter cake is dried at 105°C to a constant weight, the weight difference is measured, and the moisture content (Wc) of the filter cake is calculated.

[0062] The results are as follows Fig. 9 As shown in the figure, when the sludge pH value is in the range of 2 to 6, with the increase of pH, the sludge SRF shows a trend of first decreasing and then increasing. When the pH value is 2, the sludge SRF is 2.7×10 11 m / kg, the mud cake Wc was 74.08%, and the SRF was 2.59×10 11 m / kg, and the mud cake Wc is 70.64%. The reason for this phenomenon is that when the pH is too low, the H + The excessive content of H will neutralize the negative charge in the sludge particles, thus making the remaining H + A new repulsive force is generated between the sludge particles, the coagulation of the sludge flocs is hindered, and the construction of the sludge dewatering channel is insufficient, which affects the dewatering effect of the overall sludge system. + It is not enough to neutralize the negative charge between the sludge flocs, so that some sludge flocs cannot be completely broken up. It also affects the operation of the FeMo-BC / PMS / TA system, and the sludge dewatering effect is not ideal.

[0063] Example 10 Effect of reaction time on sludge dehydration The method and steps are the same as those in Example 9. The pH in step (1) is adjusted to 4, and then the stirring reaction time in step (2) is controlled at 10 min, 20 min, 30 min, 40 min and 50 min, respectively, to complete the conditioning and detect the corresponding indicators.

[0064] The results are as follows Fig.10 As shown in the figure, the sludge SRF and mud cake Wc showed a gradual downward trend with the extension of conditioning time. When the conditioning time was 30 min, the sludge SRF was 2.59×10 11m / kg, the mud cake Wc was 70.64%. The sludge SRF and mud cake Wc did not decrease significantly when the conditioning time was extended to 50min, indicating that FeMo-BC can quickly catalyze PMS to achieve oxidation and decomposition of sludge flocs. Therefore, the optimal conditioning time is 30min, under which PMS can be quickly catalyzed to achieve sludge conditioning and avoid the loss of cohesion of sludge flocs, resulting in reduced sludge dewatering effect.

[0065] Example 11 Effects of different substances on sludge dewatering (1) At room temperature, the sludge was fully stirred and the pH value was adjusted to 4, and then evenly divided into multiple groups; (2) Add corresponding solid substances to the four groups of sludge for conditioning. The specific addition conditions are as follows: RS group: no solid matter was added; FeMo-BC / PMS / TA group (system A): FeMo-BC, PMS and TA were added to the sludge to a concentration of 100 mg / g, 40 mg / g and 40 mg / g, respectively; Fe-BC / PMS / TA group (system B): Fe-BC, PMS and TA were added to the sludge to a concentration of 100 mg / g, 40 mg / g and 40 mg / g, respectively; Mo-BC / PMS / TA group (system C): Mo-BC, PMS and TA were added to the sludge to make their concentrations 100 mg / g, 40 mg / g and 40 mg / g respectively; the preparation method of Mo-BC was as follows: bamboo powder was mixed with water and dried, and then pyrolyzed at 550°C in a nitrogen atmosphere to obtain BC, and then BC was mixed with sodium molybdate and thiourea for hydrothermal reaction at 180°C for 10 hours, and Mo-BC was obtained after washing and drying; FeMo-BC / PMS group (system D): FeMo-BC and PMS were added to the sludge to a concentration of 100 mg / g and 40 mg / g, respectively; BC / PMS / TA group (system E): BC, PMS and TA were added to the sludge to a concentration of 100 mg / g, 40 mg / g and 40 mg / g, respectively; PMS group (system F): PMS was added to the sludge to a concentration of 40 mg / g; TA group (system G): TA was added to the sludge to a concentration of 40 mg / g; (3) The above-mentioned groups of sludge were stirred at 120 r / min for reaction, and the conditioning was completed after 30 minutes and the corresponding indicators were tested.

[0066] The results are as follows Fig.11As shown in the figure, different systems for conditioning sludge produce different sludge dewatering effects. The SRF of the unconditioned raw sludge is 9.77×10 11 m / kg, the sludge cake Wc is 85.68%. The sludge SRF after conditioning in system G is 5.12×10 11 m / kg, with a decrease rate of 47.5%; the mud cake Wc decreased to 79.24%, with a decrease rate of 7.51%, indicating that TA effectively combined with macromolecular biopolymers through bridging complexation during sludge dewatering, thereby causing the EPS protein in the sludge to precipitate. This mechanism significantly promoted the overall dewatering effect of the sludge. The SRF of the sludge after conditioning with system E was reduced to 7.11×10 11 m / kg, with a decrease rate of 27.22%; the mud cake Wc was 82.59%, with a decrease rate of 3.6%. Both decrease rates were lower than those of PMS alone. This is because bamboo charcoal without any metal particles only plays a role in skeleton construction during sludge conditioning and cannot activate PMS. At the same time, the addition of TA will slightly inhibit the activation reaction of PMS alone, resulting in a decrease in sludge dewatering effect. The SRF of sludge conditioned by system D was reduced to 5.09×10 11 m / kg, the Wc of the mud cake was reduced to 78.32%, indicating that the Fe3O4 loaded on FeMo-BC would activate PMS, causing PMS to release sufficient free radicals and promote the destruction of sludge EPS. The SRF of the sludge conditioned by system C was reduced to 4.64×10 11 m / kg, the mud cake Wc dropped to 73.67%, which was lower than the sludge SRF conditioned by system B, which was 5.06×10 11 m / kg and sludge cake Wc is 74.12%. Since the molybdenum loading is lower than the iron loading, it can be inferred that the catalytic activity of molybdenum may be stronger than that of iron in catalyzing PMS for sludge dewatering. By comparing system A with system B and system C, it can be seen that the bamboo charcoal with dual loading of iron and molybdenum is more catalytic than the bamboo charcoal with either of them loaded alone. This is because the catalyst with dual metal loading has more active sites on the surface, so the catalytic performance is stronger in the reaction system, which further improves the sludge dewatering effect.

[0067] Example 12 Effects of different substances on EPS in sludge conditioning (1) Take the conditioned sludge in the FeMo-BC / PMS / TA group (system A), FeMo-BC / PMS group (system D), PMS group (system F), and TA group (system G) in Example 11, centrifuge and retain the sludge, rinse with distilled water, add 0.05% 60°C sodium chloride solution to resuspend, keep warm for 1 hour, cool to room temperature, and centrifuge to retain the supernatant as the EPS solution; (2) The protein content in the EPS solution was determined by the Coomassie Brilliant Blue G250 method, and the polysaccharide content in the EPS solution was determined by the anthrone-sulfuric acid method.

[0068] The results are as follows Fig.12 As shown in figure a, compared with the RS group, the TA group reduced the protein contents in S-EPS, LB-EPS, and TB-EPS by 58.33%, 65.11%, and 38.78%, respectively. This is because TA can effectively complex and precipitate proteins. In the FeMo-BC / PMS group, the total protein content in EPS decreased, among which the protein content in TB-EPS decreased significantly, but the protein content in S-EPS increased. This is because the oxidation and decomposition of TB-EPS released part of the protein into S-EPS, and the addition of catalysts and oxidants could not complex and precipitate the protein, which led to a slight increase in the protein content in the S-EPS layer. In the FeMo-BC / PMS / TA group, the protein content in the S-EPS, LB-EPS, and TB-EPS layers decreased by 68.75%, 76.74%, and 77.55%, respectively. This is because a large amount of protein was released from the EPS after oxidation and decomposition, which was further complexed and precipitated by TA, thereby significantly reducing the protein content in each layer of EPS. It shows that the FeMo-BC / PMS / TA system can effectively destroy the sludge floc structure and release protein, which is beneficial to the improvement of sludge dewatering performance.

[0069] The influence of different conditioning systems on the content of polysaccharides in EPS is similar to that of proteins. The polysaccharide content of each layer of EPS in the TA group decreased significantly; in the FeMo-BC / PMS / TA group, except for a slight increase in the polysaccharide content in S-EPS, the polysaccharide content in LB-EPS and TB-EPS decreased significantly; in the FeMo-BC / PMS / TA group, the polysaccharide content in S-EPS, LB-EPS, and TB-EPS decreased by 60.21%, 71.05%, and 72.22%, respectively ( Fig.12 b), indicating that the combined conditioning of sludge with FeMo-BC / PMS / TA can more effectively break up the floc structure and reduce the polysaccharide content in EPS.

[0070] Embodiment 13 (1) The conditioned wastewater in the RS group and the FeMo-BC / PMS / TA group in Example 11 was filtered, freeze-dried, and photographed under an electron microscope; (2) The conditioned wastewater in the RS group and the FeMo-BC / PMS / TA group in Example 11 was filtered to obtain a mud cake, and then the mud cake was subjected to X-ray diffraction analysis.

[0071] Electron microscopy results Fig.13As shown in the figure, the unconditioned sludge in the RS group aggregated into clumps with a smooth and dense surface, making it difficult for the water wrapped inside the sludge particles to escape, which is not conducive to the deep dehydration of the sludge; while the sludge in the FeMo-BC / PMS / TA group was obviously broken, and the original tight clumping structure collapsed to form a pore structure. The pore structure provided more water passages for the water to escape during the sludge filtration process, which was conducive to the release of internal water and promoted the deep dehydration of the sludge.

[0072] X-ray analysis results show that the main mineral composition of the mud cake of RS group is SiO2, while CaSO4 and NaFeSi2O6 appear in the mud cake of FeMo-BC / PMS / TA group, indicating that SO4 generated by FeMo-BC activated PMS - ·Converted into SO4 after oxidation of sludge flocs 2- , and the Ca 2+ Combined to form CaSO4, while FeMo-BC activated PMS and formed Fe 3+ The Na originally existing in the sludge system + With SiO3 2- Combined to form NaFeSi2O6 ( Fig.14 ). Therefore, during the sludge conditioning process, the FeMo-BC / PMS / TA system breaks down the sludge flocs through redox reactions, and the generated CaSO4 and NaFeSi2O6 can be used as the skeleton material of the sludge dewatering channel, promoting the removal of water from the sludge and improving the sludge dewatering performance.

Claims

1. An application of FeMo-BC, characterized in that: The application is application in sludge conditioning.

2. The use of FeMo-BC according to claim 1, characterized in that: The conditioned sludge refers to the water content and / or sludge specific resistance of the conditioned sludge.

3. The use of FeMo-BC according to claim 2, characterized in that: The water content of the sludge is conditioned by adjusting CST and / or mud cake Wc and degrading flocculated EPS.

4. The use of FeMo-BC according to claim 1, characterized in that: The application is to use Fe3O4 / MoS2 modified biochar, PMS and TA to jointly condition sludge.

5. The use of FeMo-BC according to claim 4, characterized in that: The mass ratio of the FeMo-BC, PMS and TA is 8-15:2-6:2-6.

6. The use of FeMo-BC according to claim 5, characterized in that: The mass ratio of the FeMo-BC, PMS and TA is 10:4:

4.

7. The use of FeMo-BC according to claim 4, characterized in that: The total amount of FeMo-BC, PMS and TA used in the combined sludge conditioning is 10%-25% of the dry weight of the sludge.

8. The use of FeMo-BC according to claim 4, characterized in that: The combined conditioning time is 20-50 minutes, the combined conditioning pH value is 2-6, and the combined conditioning rotation speed is 100-150r / min.

9. A method for preparing FeMo-BC according to any one of claims 1 to 8, characterized in that: The steps include: (1) Dissolving biomass powder and ferrate in water, stirring evenly, drying, and pyrolyzing under an inert atmosphere to obtain Fe-BC; (2) Fe-BC is mixed with molybdate, a sulfur-containing reducing agent and water, and after hydrothermal reaction, the mixture is centrifuged, washed and dried to obtain FeMo-BC.

10. The preparation method according to claim 9, characterized in that: The biomass powder in step (1) is bamboo powder; the mass ratio of Fe-BC to molybdate in step (2) is 1-2:1-3; The pyrolysis temperature in step (1) is 450-650°C; In step (2), the mass ratio of molybdate to sulfur-containing reducing agent is 1:2; The hydrothermal reaction conditions in step (2) are 160-200° C. for 8-14 hours.

Citation Information

Patent Citations

  • A natural polysaccharide modified biological iron-based catalytic material and its preparation method and application

    CN117654625B

  • Biological excess sludge deep dehydration conditioner

    CN105753296A

  • Preparation method of heterogeneous Fenton catalyst Fe3C / C composite material

    CN108404947A

  • Graphitized porous biochar, and method for degrading organic pollutants in water body by using graphitized porous biochar

    CN109292883A

  • Deep dewatering method for sludge