Novel professional decoration cement and preparation method thereof
By optimizing the composition of cement clinker and additives, we have solved the problems of high grade and high cost of existing decoration cement, and prepared a new type of professional decoration cement that is safe, low-cost and has good water retention, avoiding tile shedding and environmental hazards, and improving the quality of decoration. Decoration quality and economic benefits.
Patent Information
- Application Number
- CN202411179171.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-27
- Publication Date
- 2024-10-11
AI Technical Summary
The decoration cement in the existing market has problems such as cracking, hollowing, and falling off of ceramic tiles due to excessively high markings. At the same time, the cost is high and some companies use materials that do not meet regulations, resulting in potential harm to the environment and human health.
A new type of professional decoration cement is made by mixing and grinding cement clinker, desulfurization gypsum, limestone, fly ash and slag powder in specific proportions. By optimizing the composition and adding liquid grinding aids, the specific surface area and water retention rate are increased. Reduce heavy metal content and radiation to ensure construction safety and economy.
A new type of professional decoration cement that is safe, low-cost and has good water retention has been realized, which avoids the falling off of ceramic tiles and environmental hazards, and improves the decoration quality and economic benefits.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cement production, and in particular to a novel professional decoration cement and a preparation method thereof. Background Art
[0002] The new professional decoration cement is a hydraulic cementitious material with good water retention and suitable mortar fluidity, made of two or more active mixed materials or industrial waste with hydraulic properties and harmful substance content that meets the specified requirements as the main raw materials, with appropriate amounts of silicate cement clinker and gypsum added, and ground into a fine powder. At present, the cement used for decoration in the market is generally general-purpose silicate cement, which has a high grade, resulting in cracking, hollowing, and falling of tiles during decoration. At the same time, the cost of general-purpose silicate cement is relatively high. In order to reduce costs, some companies use materials that do not meet the regulations, resulting in excessive radioactivity and hexavalent chromium in cement, which is a water-soluble heavy metal, posing potential hazards to the environment and the health of construction workers. How to balance cost and quality safety has become a major problem. Summary of the invention
[0003] In order to solve the above technical problems, the present invention provides a new type of professional decoration cement and a preparation method thereof. The prepared new type of professional decoration cement is safe, low in cost, has good water retention performance and good mortar fluidity.
[0004] To achieve this technical purpose, the present invention adopts the following scheme: In a first aspect, the present invention provides a new type of professional decoration cement, which is made of the following raw materials by mass: 25-30 parts of cement clinker, 4 parts of desulfurized gypsum, 25 parts of limestone, 15-20 parts of fly ash, 25-26 parts of slag powder, and 0.02 parts of liquid grinding aid.
[0005] Preferably, the new professional decoration cement is made from the following raw materials by mass: 29 parts of cement clinker, 4 parts of desulfurized gypsum, 25 parts of limestone, 17 parts of fly ash, 25 parts of slag powder, and 0.02 parts of liquid grinding aid.
[0006] Preferably, the cement clinker comprises the following components by mass: 45-55 parts of tricalcium silicate, 18-28 parts of dicalcium silicate, 6-10 parts of tricalcium aluminate, and 11-13 parts of tetracalcium aluminoferrite.
[0007] Preferably, the moisture content of the desulfurized gypsum is 13-20%, the chloride ion content is 0.05-0.3%, and the SO3 content is 35-40%.
[0008] Preferably, the moisture content of the desulfurized gypsum is 18%, the chloride ion content is less than 0.1%, and the SO3 content is 40%.
[0009] Preferably, the fly ash has no irritating odor, an ammonium ion content of 0-100 mg / kg, and an activity of more than 70% after 28 days.
[0010] Preferably, the chloride ion content of the slag powder is ≤0.06%, and the 28-day activity is >100%.
[0011] Preferably, the liquid grinding aid is an alcoholamine compound.
[0012] Preferably, the liquid grinding aid is an alcoholamine compound with triethanolamine as the main material.
[0013] Preferably, the liquid grinding aid is a 3W model produced by Jinyu Technology Co., Ltd.
[0014] In the second aspect, the present invention also provides a method for preparing a novel professional decoration cement, wherein cement clinker, desulfurized gypsum, limestone, liquid grinding aid, and fly ash are mixed and ground into a powdery material of a certain fineness, slag powder is added and mixed when passing through a finished product chute, and the mixture is stirred evenly to prepare a novel professional decoration cement having a specific surface area of ≥450m 2 / kg; 45μm fineness ≤5.0%.
[0015] Compared with the prior art, the present invention has the following beneficial effects: 1. The dosage of desulfurized gypsum is fixed, the SO3 content in cement is stabilized at about 1.90%, and the initial setting time of cement is about 180 minutes, which is the most suitable time during the decoration construction process.
[0016] 2. The present invention uses 25% slag powder, which increases the specific surface area of cement, can improve the water retention rate of the cement, and also reduces the amount of clinker, reduces the heavy metal content and radiation brought into the clinker, and is very safe for human contact during home decoration. In addition, with the addition of slag powder, the durability of cement is improved, and the decoration quality is improved.
[0017] 3. The present invention uses 25% high-quality limestone, which can improve the three-day compressive strength of cement, and has a great advantage in improving the progress of decoration.
[0018] The novel professional decoration cement of the present invention is characterized by low heavy metal content, low radioactivity, high water retention rate, low construction cost, good decoration effect, and especially can avoid potential harm to human body and ecological environment protection, and can be promoted and applied in home decoration projects.
[0019] The present invention optimizes the composition of the mixed materials, ensures that the compressive strength and bonding ability of the cement meet the construction requirements when the amount of cement clinker is small, and improves the water retention rate of the cement, which is convenient for on-site construction of the cement. Even if watering and curing are occasionally forgotten, the hydration reaction can be completed by relying on the moisture in the mortar, and problems such as strength reduction and tile shedding due to water loss due to drying will not occur. In addition, the new professional decoration cement of the present invention has low cost and has better performance and economic and environmental benefits than traditional general-purpose silicate cement. DETAILED DESCRIPTION
[0020] In order to fully understand the purpose, features and effects of the present invention, the present invention is described in detail through the following specific implementation methods, but the present invention is not limited thereto.
[0021] In the present invention, the materials used are all commercially available unless otherwise specified. Among them, the moisture content of desulfurized gypsum is 18%, the chloride content is less than 0.1%, and the SO3 content is 40%; the fly ash has no irritating odor, the ammonia content of the fly ash is less than 100 mg / kg, and the 28-day activity is greater than 70%; the chloride content of the slag powder is ≤0.06, and the 28-day activity is greater than 100%.
[0022] Cement clinker is a raw material powder with a certain fineness that is ground into a certain proportion of calcium material, aluminum material, iron material, and silicon material. After preheating, it is put into a rotary kiln for calcination and cooling to obtain a material with tricalcium silicate, dicalcium silicate, tetracalcium aluminoferrite and tricalcium aluminate as the main minerals. Cement clinker includes the following components by mass: 48 parts of tricalcium silicate, 25 parts of dicalcium silicate, 7 parts of tricalcium aluminate, and 12 parts of tetracalcium aluminoferrite.
[0023] The present invention provides a novel professional decoration cement and a preparation method thereof, and specific embodiments are as follows. Example 1
[0024] A new type of professional decoration cement is prepared according to the following steps: 29 parts of cement clinker, 4 parts of desulfurized gypsum, 25 parts of limestone, 17 parts of fly ash and 0.02 parts of liquid grinding aid are mixed and then passed through a roller press into a mill. After being ground and sorted in the mill, it enters the finished product chute. When passing through the finished product chute, it is mixed with 25 parts of slag powder and mixed evenly in a mixer to produce a new type of professional decoration cement with a specific surface area of ≥450m 2 / kg; 45μm fineness ≤5.0%. Specific: (1) Cement clinker, desulfurized gypsum, limestone and liquid grinding aid are measured separately in proportion, mixed and then put into the mill for grinding; (2) Fly ash is added into the mill from the grinding head according to the proportion and mixed and ground; (3) Grind the mixed raw material powder multiple times through a roller press, a ball mill and a high-efficiency powder concentrator, and add a specified proportion of slag powder into the finished product chute; (4) The mixed materials are then mixed evenly in a mixer to obtain a new type of professional decoration cement product, with a fineness of 45μm ≤5%.
[0025] Examples 2 to 5 and Comparative Examples 1 to 3
[0026] The preparation methods of Examples 2 to 5 and Comparative Examples 1 to 3 are the same as that of Example 1, and the raw material ratios are shown in the following table:
[0027] To illustrate the beneficial effects of the present invention in more detail, the results of different tests are analyzed as follows: The test is based on GB175-2007 "General Portland Cement". The test results are shown in the table below.
[0028]
[0029] In this test, Examples 1 to 5 have good water retention performance, low radioactivity and low cost, among which Examples 2 to 5 have relatively poor compressive performance, and Example 1 has good compressive performance.
[0030] Comparative Examples 1 to 3 are compared with Example 1. Under the premise of increasing the clinker by 3% and keeping the same gypsum ratio, the 3-day strength is basically the same by reducing the limestone, fly ash and slag powder by the same amount, and the 28-day strength is reduced to varying degrees. At the same time, the material cost is also increased by 2-5 yuan / ton accordingly. Therefore, Example 1 is the optimal solution in terms of quality and cost.
[0031] The fluidity of the cement mortar in Examples 1 to 5 was tested, and the test result was 230±10 mm. When prepared into mortar, the mortar consistency was tested to be 78±2 mm, and all had excellent construction performance.
[0032] The new professional cement of the present invention has a low clinker content. As the content of cement clinker decreases, the compressive performance decreases, but still achieves a good compressive strength, can meet the construction requirements, and has a high economic benefit. In Example 1, only 29% of the cement clinker content can reach a strength of about 16.0MPa, which is a very cost-effective choice for daily decoration. In addition, the amount of cement clinker used in the present invention is less, and the cost is as low as 103.19 yuan / ton. Compared with the cost of about 200 yuan of ordinary Portland cement, the cost is reduced a lot, and the content of various harmful indicators is low, avoiding the current human body harm.
[0033] In summary, the present invention does not add chemical substances such as powder enhancers and mineralizers, but only adds a small amount of liquid grinding aids (alcoholamine substances) to reduce the introduction of chemical raw materials into cement. Through the mixed material compounding, it is ensured that the compressive strength of cement meets the construction requirements, and at the same time, the water retention rate of cement is improved, which is convenient for on-site construction of cement. Even if watering and curing are occasionally forgotten, the hydration reaction can be completed by the mortar water, and the problems such as strength reduction and tile falling off due to drying and water loss will not occur. In addition, the new professional decoration cement of the present invention has low cost and better performance and economic and environmental benefits than traditional general-purpose silicate cement.
[0034] Finally, it should be noted that the above are only preferred embodiments of the present invention. Of course, those skilled in the art can make changes and modifications to the present invention. If these modifications and variations fall within the scope of the claims of the present invention and their equivalent technologies, they should be considered to be within the scope of protection of the present invention.
Claims
1. A new type of professional decoration cement, It is characterized in that It is made of the following raw materials by mass: 25-30 parts of cement clinker, 4 parts of desulfurized gypsum, 25 parts of limestone, 15-20 parts of fly ash, 25-26 parts of slag powder, and 0.02 parts of liquid grinding aid.
2. The new professional decoration cement according to claim 1, It is characterized in that It is made from the following raw materials by mass: 29 parts of cement clinker, 4 parts of desulfurized gypsum, 25 parts of limestone, 17 parts of fly ash, 25 parts of slag powder, and 0.02 parts of liquid grinding aid.
3. The new professional decoration cement according to claim 1, It is characterized in that The cement clinker comprises the following components by mass: 45-55 parts of tricalcium silicate, 18-28 parts of dicalcium silicate, 6-10 parts of tricalcium aluminate, and 11-13 parts of tetracalcium aluminoferrite.
4. The new professional decoration cement according to claim 1, It is characterized in that The moisture content of desulfurized gypsum is 13~20%, the chloride ion content is 0.05~0.3%, and the SO 3 It is 35~40%.
5. The new professional decoration cement according to claim 1, It is characterized in that Fly ash has no irritating odor, an ammonia ion content of 0~100 mg / kg, and an activity of >70% after 28 days.
6. The new professional decoration cement according to claim 1, It is characterized in that The chloride ion content of slag powder is ≤0.06%, and the activity after 28 days is >100%.
7. The new professional decoration cement according to claim 1, It is characterized in that The liquid grinding aid is an alcoholamine compound.
8. The new professional decoration cement according to claim 7, It is characterized in that The liquid grinding aid is an alcoholamine compound with triethanolamine as the main material.
9. A method for preparing the new professional decoration cement according to any one of claims 1 to 6, It is characterized in that Cement clinker, desulfurized gypsum, limestone, liquid grinding aid and fly ash are mixed and ground into powdery materials of a certain fineness. Slag powder is added and mixed when passing through the finished product chute. The mixture is stirred evenly to produce a new type of professional decoration cement with a specific surface area of ≥450m 2 / kg; 45μm fineness ≤5.0%.
Citation Information
Patent Citations
Green low-carbon cement for roadbed and preparation method of green low-carbon cement
CN117164258A