All-solid-waste-based cementing material for stabilizing aeolian sand as well as preparation method and application of all-solid-waste-based cementing material
By using all-solid waste-based cementitious materials in aeolian sand and using alkaline solid waste to provide a reaction environment, sulfates and silica-aluminum solid waste can self-spark chemical reactions, solving the problem of poor stability and high cost of aeolian sand roadbed. solve the problem and achieve the low-cost, environmentally friendly and efficient reinforcement effect of the material, which is suitable for desert highway construction.
Patent Information
- Application Number
- CN202410966967.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
AI Technical Summary
The application of aeolian sand as road material reinforcement and improvement has problems of poor stability and high cost. Traditional alkali-activated solid waste cementitious materials have shortcomings in construction safety and environmental safety, and can easily lead to drying shrinkage and crack diseases.
Common alkaline bulk industrial solid waste, sulfate solid waste and silica-aluminum solid waste are used to develop all-solid waste-based cementitious materials through orthogonal experiments. The alkaline solid waste is used to provide a reaction environment to make sulfate and silica-aluminum solid waste. The solid waste self-stimulates to produce chemical reactions, condenses wind-deposited sand particles, reduces costs and environmental risks, and replaces cement and alkali-activated cementitious materials.
It improves the strength and stability of the aeolian sand roadbed, reduces material costs and environmental safety risks, simplifies the production process, has a wide range of applications, can absorb industrial solid waste on a large scale, reduces carbon emissions, and is suitable for desert highway construction.
Smart Images

Figure CN118754531A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of highway materials, and in particular to a full-solid waste-based cementitious material for stabilizing aeolian sand, and a preparation method and application thereof. Background Art
[0002] Deserts are widely distributed in my country and around the world, with a total area of more than 31 million km 2 , accounting for one-fifth of the total land area; my country's desert area is as high as 1.3 million km 2 , accounting for about one-seventh of the country's total land area. Using aeolian sand as a road construction material to build roadbeds or base layers in desert areas that lack high-quality fillers can not only save costs by using local materials, but also has great environmental benefits. However, the properties of aeolian sand, such as poor grading, lack of cohesion, poor shear resistance and poor stability, make the aeolian sand roadbed prone to instability damage; and currently, traditional inorganic binders such as cement and lime are mainly used to improve aeolian sand to improve the strength and stability of aeolian sand roadbed, but the use of inorganic binders with strong hydration properties will lead to more significant road temperature and shrinkage cracking diseases, and will increase the cost of the project. Therefore, the application research of aeolian sand as a road material reinforcement and improvement has become one of the urgent problems to be solved in desert highway construction.
[0003] At the same time, the annual output of bulk industrial solid waste in my country has reached 4 billion tons, and the historical stockpile has exceeded 70 billion tons, which has posed new challenges to ecological environmental protection and industrial structure adjustment, making the elimination of solid waste in various industries an urgent and important task. The use of industrial solid waste to develop building materials is a research hotspot in the current engineering industry, especially in the field of highway construction, which can closely meet the needs of road engineering construction for the large consumption of mineral resources and the green, low-carbon and sustainable development concept. Studies have shown that all-solid waste-based cementitious materials, as a new type of cementitious material, have the advantages of controllable compressive strength, adjustable setting time, wide range of applications, low material cost, energy saving and environmental protection when used to stabilize road construction materials. Application research has been widely carried out throughout the country. However, there are few reports on the research of all-solid waste-based road cementitious materials, especially the research on all-solid waste cementitious materials used to reinforce aeolian sand.
[0004] At present, the research on solid waste-based cementitious materials mainly adopts alkali activation or acid activation, using kaolin or potentially active silicon and aluminum oxides as precursor materials, and generating hydrated aluminosilicate crystals through alkali activation to produce chemical reactions, thereby improving the mechanical strength of the system. However, alkali-activated solid waste cementitious materials also have some disadvantages: there are few application scenarios in actual road projects, and alkali activators mostly use NaOH, KOH or sodium silicate aqueous solutions. Chemical solutions with strong alkalinity are not only expensive and increase costs, but also have low construction safety and environmental safety, which limits their promotion and application; at the same time, alkali-activated cementitious materials show more significant drying shrinkage and cracking, especially in desert areas with little rainfall, strong evaporation, and large temperature differences. The solidification of stable aeolian sand will aggravate the generation and development of crack-type diseases under the coupling of environmental loads. Summary of the invention
[0005] In view of the deficiencies of the above-mentioned prior art, the purpose of the present invention is to provide a fully solid waste-based cementitious material for stabilizing aeolian sand, and a preparation method and application thereof. The present invention proposes to utilize common alkaline bulk industrial solid waste, sulfate solid waste and silicoaluminous solid waste, and develop a new type of fully solid waste road cementitious material through orthogonal experiment, and stabilize the aeolian sand roadbed and base with a large amount of solid waste-based cementitious material, so as to accelerate the construction of desert highways and consume a large amount of bulk industrial solid waste, provide reliable technical support for the construction of low-carbon green desert highways, and ensure the safety, stability and sustainable development of the project.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] A fully solid waste-based cementitious material for stabilizing aeolian sand, the fully solid waste-based cementitious material comprising the following raw materials in parts by weight:
[0008] 50-90 parts of aeolian sand material, 10-50 parts of industrial solid waste gelling material and water, wherein the mass percentage of the industrial solid waste gelling material in the solid raw material of the all-solid waste-based gelling material is 10-50%, and the mass ratio of water in the aeolian sand material and the industrial solid waste gelling material is 14%-17%;
[0009] The industrial solid waste gelling material includes alkaline solid waste, sulfate solid waste and silicon-aluminum solid waste;
[0010] In a preferred embodiment of the present invention, the alkaline solid waste is carbide slag, the sulfate solid waste is desulfurization gypsum, the siliceous and aluminous solid waste is fly ash, silica ash, and blast furnace slag powder, and the industrial solid waste materials are ground to a mesh size greater than or equal to 200 mesh; carbide slag and desulfurization gypsum are easy to agglomerate when leaving the factory and should be dried before grinding; fly ash, silica ash and blast furnace slag powder have sufficient fineness when leaving the factory but should be dried before use.
[0011] In a preferred embodiment of the present invention, the mass ratio of carbide slag, desulfurization gypsum, fly ash, silica ash and blast furnace slag powder is 4:2:2:3:2.
[0012] In a preferred embodiment of the present invention, the siliceous and aluminous solid waste also includes coal gangue powder.
[0013] Another object of the present invention is to provide a method for preparing the all-solid waste-based cementitious material for stabilizing aeolian sand as described in any one of the above, comprising the following steps:
[0014] Weigh the following raw materials in parts by weight: 50-90 parts of aeolian sand material, 10-50 parts of industrial solid waste gelling material and water, the mass percentage of industrial solid waste gelling material in the solid raw materials of the all-solid waste-based gelling material is 10-50%, the mass ratio of water in the aeolian sand material and the industrial solid waste gelling material is 14%-17%, wherein the mass ratio of carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in the industrial solid waste gelling material is 4:2:2:3:2;
[0015] Carbide slag, desulfurized gypsum, fly ash, silica ash and blast furnace slag powder are mixed in a mass ratio of 4:2:2:3:2 to obtain a dry industrial solid waste gel material;
[0016] Adding the aeolian sand material to the dry material of the industrial solid waste gel material, stirring and mixing to obtain a mixed dry material of the solid waste gel material and the aeolian sand;
[0017] Adding 30-50% of water by a predetermined weight to the mixed dry material of the solid waste cementitious material and the aeolian sand, stirring and mixing, and then suffocating the material;
[0018] Finally, the remaining water is added, stirred again, and statically pressed to obtain a fully solid waste-based cementitious material.
[0019] In a preferred embodiment of the present invention, the static pressure forming stabilization time is 1 to 2 hours.
[0020] In a preferred embodiment of the present invention, the stewing time is 6 to 12 hours.
[0021] The third object of the present invention is to provide an application of the all-solid waste cementitious material described in any one of the above items in stabilizing aeolian sand roadbed and base.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] 1. The present invention provides an all-solid waste cementitious material for stabilizing aeolian sand. It does not use admixtures for excitation, optimizes the material composition design, accelerates the recycling of solid waste materials, and provides a reaction environment through alkaline solid waste materials, so that sulfate solid waste and silicon-aluminum solid waste can self-excite to produce a lasting chemical reaction to condense aeolian sand particles, thereby reducing material costs and environmental safety risks. The solid waste material ratio is improved and determined through orthogonal experimental design, thereby improving the feasibility and diversity of the material ratio to meet different application scenarios, thereby being able to replace cement and alkali-activated cementitious materials to stabilize aeolian sand.
[0024] 2. The all-solid waste cementitious material provided by the present invention to improve the aeolian sand base layer can improve strength and stability, reduce the height of the traditional water-stabilizing layer, and improve toughness; and the production process of the all-solid waste cementitious material is simple, and can utilize large amounts of industrial solid waste and aeolian sand resources nearby on a large scale, with significant economic benefits.
[0025] 3. The all-solid waste cementitious material of the present invention can replace cement and reduce the amount of cement used in road projects. At the same time, it can recycle and utilize industrial solid waste in large quantities, effectively reduce carbon emissions and alleviate environmental pollution. This technology can provide important theoretical and practical support for the design and construction of solidified aeolian sand base projects, guide the reasonable evaluation and effective control of the application of aeolian sand base in engineering practice, and improve the quality and safety of the project. Compared with traditional alkali excitation technology, a large amount of all-solid waste cementitious material can absorb large amounts of industrial solid waste on a large scale. Its application in road projects can effectively alleviate the pressure of solid waste emissions, eliminate disposal costs, and promote the development of social industrial economy. The all-solid waste cementitious material has a wide range of applications and provides a reference for similar roadbed treatment and other industries. It is of great significance to promote the green transformation of related industries. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a schematic diagram of the proportion of each solid material in the orthogonal test of the present invention;
[0027] Figure 2 The results of the 7-day unconfined compression test of the orthogonal test of the present invention;
[0028] Figure 3 The sensitivity analysis results of various solid waste materials in the present invention;
[0029] Figure 4 The compaction test results of the solid waste cementitious material admixture of the present invention;
[0030] Figure 5 This is a relationship diagram between the age and the unconfined compressive strength under the dosage of the solid waste cementitious material of the present invention;
[0031] Figure 6 This is a relationship diagram between the age and the unconfined compressive strength at a solid waste cementitious material dosage of 30% according to the present invention;
[0032] Figure 7 This is a relationship diagram between compaction degree and unconfined compressive strength at 30% solid waste cementitious material dosage of the present invention;
[0033] Figure 8 This is a relationship diagram between the amount of solid waste cementitious material added and the internal friction angle and cohesion of the present invention;
[0034] Fig. 9 The relationship diagram between the amount of solid waste cementitious material added and the CBR California bearing ratio of the present invention;
[0035] Fig.10 This is a relationship diagram between the dosage of the solid waste cementitious material and the compressive rebound modulus of the present invention;
[0036] Fig.11 This is a graph showing the relationship between the amount of solid waste cementitious material added and water stability in the present invention;
[0037] Fig.12 It is the unconfined compressive strength of the test block with a height-to-diameter ratio of 1:1 within 90 days when the solid waste cementitious material dosage is 20-30% of the present invention;
[0038] Fig.13 It is the unconfined compressive strength within 28 days of the test block with a height-to-diameter ratio of 2:1 when the solid waste cementitious material dosage is 10-40% according to the present invention. DETAILED DESCRIPTION
[0039] The following is a detailed description of the technical solutions in the embodiments of the present invention in combination with the preferred embodiments and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0040] It should be noted that all professional terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specifically stated, various raw materials, reagents, instruments and equipment used in the following embodiments of the present invention can be purchased from the market or prepared by existing methods.
[0041] Table 1 is a ratio scheme of the all-solid waste road cementitious material used for reinforcing aeolian sand in the present invention, and the specific steps are as follows:
[0042] S1. First, the basic physical and chemical properties of raw materials are tested, the mass ratio of aeolian sand is fixed, and the mixing ratio of all-solid waste cementitious materials is configured by orthogonal test. Under different mixing conditions, the 7d unconfined compressive strength is used as an indicator for measurement. The influence of different solid waste raw materials under this material combination is determined by linear regression analysis, and then the optimal mixing ratio combination is determined.
[0043] The S1 comprises the following steps:
[0044] S11, the mass ratio of aeolian sand is selected to be 60%, and the remaining 40% is all solid waste mixed cementitious materials. The solid waste cementitious materials are designed through a six-factor three-level orthogonal table to form 18 groups of proportions, as shown in Table 1 and Figure 1 As shown;
[0045] S12, according to the mass fraction, add carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder into the agitator in proportion, in no particular order, start the agitator, and stir for no less than 5 minutes. After the stirring is completed, the dry material of industrial solid waste cementitious material is obtained;
[0046] S13, then adding a predetermined amount of aeolian sand and stirring again for not less than 5 minutes, and mixing evenly to obtain a mixed dry material of solid waste cementitious material and aeolian sand;
[0047] S14, then add 30-50% of the predetermined mass of water, stir for not less than 5 minutes, stir evenly and put into a sealed plastic bag for 6-12 hours to keep the material stuffed;
[0048] S15. Finally, add the remaining water and stir for another 5 minutes. Add 205g of wet soil sample of each proportion into a 50×50mm cylindrical mold to form a UCS test block by static pressure. After the molding is stable for 1 to 2 hours, demould it and move it to a curing box for curing.
[0049] S16. After the predetermined age, test the unconfined compressive strength for 7 days. Figure 2 As shown in the figure, the sensitivity of each solid waste material is calculated by linear regression method, as shown in the figure. Figure 3 As shown, the best ratio is determined;
[0050] S17. Through calculation, we can know the optimal dosage level of five kinds of solid waste materials, namely, carbide slag: desulfurization gypsum: fly ash: silica ash: blast furnace slag powder = 30.7%: 15.4%: 15.4%: 23.1%: 15.4%.
[0051] S2. Carry out compaction test on the obtained mix ratio to determine the maximum dry density and optimum moisture content of aeolian sand improved by different amounts of solid waste cementitious materials, and test the strength of different amounts, different ages and different compaction degrees.
[0052] The S2 comprises the following steps:
[0053] S21. Compaction test: Heavy compaction test, the number of compaction under different water content is not less than 5, find out the best water content and maximum dry density, such as Figure 4 As shown;
[0054] S22. When the dosage is 30%, the strength development law of the sample with a height-to-diameter ratio of 1:1 at different dosages of solid waste cementitious materials is as follows Figure 5 As shown;
[0055] S22, when the dosage is 30%, the strength development law of the specimen with a height-to-diameter ratio of 1:1 at different ages is as follows Figure 6 As shown;
[0056] S23, when the dosage is 30%, the strength variation law of the sample with a height-to-diameter ratio of 1:1 under compaction degree is as follows Figure 7 shown.
[0057] S3. Optimize the obtained mix ratio and further test the working performance, including shear strength, CBR value, compressive rebound modulus, water stability, etc.
[0058] The S3 includes the following steps:
[0059] S31, test the shear strength immediately after preparing the sample at 97% compaction. Figure 8 As shown;
[0060] S32, test the CBR value immediately after preparing the sample at 97% compaction degree. The result is as follows Fig. 9 As shown;
[0061] S33, after preparing samples at 98% compaction, curing to different ages, testing the compressive resilience modulus of the top surface method, the results are as follows Fig.10 As shown;
[0062] S34, after preparing the sample at 98% compaction, curing for 7 days, testing the ratio of 24h immersion to no immersion on the 7th day, i.e. water stability, the results are as follows Fig.11 shown.
[0063] Table 1 Orthogonal test scheme
[0064]
[0065] Example 1
[0066] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 70 parts by mass, and the remaining 30 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0067] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0068] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0069] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0070] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0071] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 50 mm cylindrical mold according to the predetermined mass of 98% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 3d, 7d, 14d, 28d, 60d and 90d respectively.
[0072] Example 2
[0073] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 75 parts by mass, and the remaining 25 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0074] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0075] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0076] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0077] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0078] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 50 mm cylindrical mold according to the predetermined mass of 98% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 3d, 7d, 14d, 28d, 60d and 90d respectively.
[0079] Example 3
[0080] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 80 parts by mass, and the remaining 20 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0081] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0082] (5) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0083] (6) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes, and mixing evenly to obtain a mixed dry material of solid waste cementitious material and aeolian sand;
[0084] (7) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0085] (8) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 50 mm cylindrical mold according to the predetermined mass of 98% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the sample was demolded and moved to a curing box for curing. The unconfined compressive strength was measured at 3 d, 7 d, 14 d, 28 d, 60 d and 90 d, respectively.
[0086] Example 4
[0087] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 60 parts by mass, and the remaining 40 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0088] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0089] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0090] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0091] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0092] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 100 mm cylindrical mold according to the predetermined mass of 97% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 0 d, 3 d, 7 d, 14 d, and 28 d, respectively.
[0093] Example 5
[0094] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 70 parts by mass, and the remaining 30 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0095] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0096] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0097] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0098] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0099] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 100 mm cylindrical mold according to the predetermined mass of 97% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 0 d, 3 d, 7 d, 14 d, and 28 d, respectively.
[0100] Example 6
[0101] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 80 parts by mass, and the remaining 20 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0102] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0103] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0104] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0105] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0106] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 100 mm cylindrical mold according to the predetermined mass of 97% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 0 d, 3 d, 7 d, 14 d, and 28 d, respectively.
[0107] Example 7
[0108] A fully solid waste-based cementitious material for stabilizing aeolian sand, comprising aeolian sand material, an industrial solid waste cementitious material and water, wherein the aeolian sand material accounts for 90 parts by mass, and the remaining 10 parts of solid materials are industrial solid waste cementitious materials, wherein the industrial solid waste cementitious materials include carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in a mass ratio of 4:2:2:3:2, and the mass ratio of water to total solids is 0.14;
[0109] The method for preparing a solid waste-based cementitious material comprises the following steps:
[0110] (1) adding carbide slag, desulfurized gypsum, fly ash, silica fume and high slag powder into a stirrer in proportion according to the mass fraction, in no particular order, starting the stirrer, stirring for no less than 5 minutes, and obtaining a dry industrial solid waste cementitious material after the stirring is completed;
[0111] (2) then adding a predetermined amount of aeolian sand and stirring again for no less than 5 minutes to obtain a mixed dry material of the solid waste cementitious material and the aeolian sand after mixing evenly;
[0112] (3) Then add 30-50% of the predetermined mass of water, stir for no less than 5 minutes, and after stirring evenly, put it into a sealed plastic bag for 6-12 hours to suffocate;
[0113] (4) Finally, the remaining water was added and stirred for another 5 min. The stirred soil sample material was added into a 50 × 100 mm cylindrical mold according to the predetermined mass of 97% compaction degree to form a UCS test block by static pressure. After the molding was stable for 1 to 2 h, the UCS test block was demoulded and moved to a curing box for curing. The unconfined compressive strength was measured at 0 d, 3 d, 7 d, 14 d, and 28 d, respectively.
[0114] Results Analysis
[0115] According to the measurement, the 7d strength of the test block with a height-to-diameter ratio of 1:1 was 2-6MPa and the 90d strength was 8-11MPa at three dosages of 20%, 25% and 30% for the solid waste cementitious material stabilized aeolian sand in Examples 1-3. The results are as follows Fig.12 As shown in JTG / T F20-2015 "Technical Specifications for Highway Pavement Base Construction" Section 4.2 p13-14, the current reference specification for the 7d-old unconfined compressive strength standard R of cement stabilized materials d The material of the present invention can be applied to different road grades and load conditions in accordance with the provisions of 4.2.4. However, cement is not used in the present invention. The strength requirements of 4.2.6 and 4.2.8 in the detailed rules are relatively low. Therefore, it can be used in the subbase of high-grade roads (expressways and first-class highways) and the base and subbase of second-class and lower roads at three dosages, indicating that the all-solid waste cementitious material stabilized aeolian sand under this ratio can be used as the base of low-grade roads or the subbase of first-class and second-class highways.
[0116] According to the measurement, when the solid waste cementitious material stabilized aeolian sand in Examples 4-7 was added in four dosages of 10% to 40%, the 7d strength of the test block with a height-to-diameter ratio of 2:1 was greater than 1MPa, and the 28d strength was 2 to 6MPa. Fig.13As shown, the main strength control index of the roadbed soil is the California bearing ratio CBR. Referring to the maximum requirement for the roadbed CBR value in P73.2.2 of JTR-D30-2015 "Standards for Highway Roadbed", which is >8%, the CBR value of the solid waste cementitious material in the present invention is greater than 100% when the content is 10% to 40%. Therefore, it can meet the requirements of roadbed filling materials, indicating that the all-solid waste cementitious material stabilized aeolian sand under this ratio can be used to fill the roadbed.
[0117] In summary, the present invention provides an all-solid waste cementitious material for reinforcing aeolian sand, which does not use admixtures for excitation, optimizes the material composition design, and accelerates the recycling of solid waste materials; provides a reaction environment through alkaline solid waste materials, so that the solid wastes can self-excite to produce a lasting chemical reaction to condense aeolian sand particles, thereby reducing material costs and environmental safety risks; improves and determines the proportion of solid waste materials through orthogonal experimental design, thereby improving the feasibility and diversity of material proportions to meet different application scenarios; and can replace cement and alkali-activated cementitious materials to stabilize aeolian sand.
[0118] It should be noted that when the present invention involves a numerical range, it should be understood that the two endpoints of each numerical range and any value between the two endpoints can be selected. Since the steps and methods used are the same as those in the embodiments, in order to avoid redundancy, the present invention describes a preferred embodiment. Although the preferred embodiments of the present invention have been described, those skilled in the art may make additional changes and modifications to these embodiments once they know the basic creative concept. Therefore, the attached claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0119] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. A solid waste-based cementitious material for stabilizing aeolian sand, characterized in that: The all-solid waste-based cementitious material includes the following raw materials in parts by weight: Solid raw materials of all-solid waste-based cementitious materials and water, wherein the solid raw materials of the all-solid waste-based cementitious materials are composed of aeolian sand materials and industrial solid waste cementitious materials, wherein the mass percentage of the industrial solid waste cementitious materials in the solid raw materials is 10-50%, and the mass percentage of water in the solid raw materials is 14%-17%; The industrial solid waste gelling material includes alkaline solid waste, sulfate solid waste and silicon-aluminum solid waste.
2. The all-solid waste-based cementitious material for stabilizing aeolian sand according to claim 1, characterized in that: Alkaline solid waste is carbide slag, sulfate solid waste is desulfurization gypsum, and siliceous and aluminous solid waste is fly ash, silica ash and blast furnace slag powder.
3. The all-solid waste-based cementitious material for stabilizing aeolian sand according to claim 2, characterized in that: Among the industrial solid waste cementitious materials, the mass ratio of carbide slag, desulfurization gypsum, fly ash, silica ash and blast furnace slag powder is 4:2:2:3:
2.
4. The all-solid waste-based cementitious material for stabilizing aeolian sand according to claim 2, characterized in that: The silicon-alumina solid waste also includes coal gangue powder, and the mass fraction of the coal gangue powder in the aeolian sand material and the industrial solid waste cementitious material is 3-6%.
5. A method for preparing a fully solid waste-based cementitious material for stabilizing aeolian sand according to claim 3, characterized in that: The following steps are involved: Weigh the following raw materials in parts by weight: aeolian sand material, industrial solid waste cementitious material and water, the mass percentage of aeolian sand material in the solid raw material of the all-solid waste-based cementitious material is 10-50%, the mass ratio of water in the aeolian sand material and the industrial solid waste cementitious material is 14%-17%, wherein the mass ratio of carbide slag, desulfurized gypsum, fly ash, silica fume and blast furnace slag powder in the industrial solid waste cementitious material is 4:2:2:3:2; Carbide slag, desulfurized gypsum, fly ash, silica ash and blast furnace slag powder are mixed in a mass ratio of 4:2:2:3:2 to obtain a dry industrial solid waste gel material; Adding the aeolian sand material to the dry material of the industrial solid waste gel material, stirring and mixing to obtain a mixed dry material of the solid waste gel material and the aeolian sand; Adding 30-50% of the predetermined mass of water to the mixed dry material of the solid waste cementitious material and the aeolian sand, stirring and mixing, and then suffocating the material; Finally, the remaining water is added, stirred again, and static pressure is applied to form a fully solid waste-based cementitious material for stabilizing aeolian sand.
6. The method for preparing the all-solid waste cementitious material for stabilizing aeolian sand according to claim 5, characterized in that: The static pressure molding stabilization time is 1 to 2 hours.
7. The method for preparing the all-solid waste cementitious material for stabilizing aeolian sand according to claim 5, characterized in that: The stuffing time is 6 to 12 hours.
8. The method for preparing the all-solid waste cementitious material for stabilizing aeolian sand according to claim 5, characterized in that: The stirring time during the preparation of all-solid waste-based cementitious materials used to stabilize aeolian sand is no less than 5 minutes.
9. Use of the all-solid waste cementitious material according to any one of claims 1 to 4 in stabilizing aeolian sand roadbed and base.
Citation Information
Patent Citations
Paste filling material composition prepared from drift-sand and industrial solid waste
CN102211916A
Aeolian sand roadbed material based on slag-fly ash geopolymer and preparation method of aeolian sand roadbed material
CN115057663A
All-solid-waste self-excitation alkaline cementing material and preparation method thereof
CN115925299A
Multi-element solid waste cementing material as well as preparation method and application thereof
CN117303770A
Production of hardened gypsum from gypsum building plates used in the building industry comprises adding a mixture of fly ash and / or wet ash to building gypsum and / or gypsum slurry to produce a moisture-resistant hardened gypsum
DE10326623A1
Cited By
Phosphogypsum and aeolian sand synergistically cured road subgrade filler and preparation method thereof
CN119707427A
All-solid waste aggregate grouting body and preparation method thereof
CN120698753A
A full-solid-waste aggregate grouting body and a preparation method thereof
CN120698753B
All-solid-waste slow-release desert sand curing agent as well as preparation method and application thereof
CN120717761A