Lithium-slag-doped offshore wind turbine foundation scouring protection sludge curing agent and preparation and application thereof

Through the composite gelling system of modified lithium slag powder, Portland cement and sulfoaluminate cement, combined with the salt-resistant tackifier of non-ionic polyacrylamide and xanthan gum, the problem of lithium slag in scour protection of offshore platforms is solved. To solve the problems of resource utilization and environmental pollution, a marine sludge solidifier with high strength, rapid solidification and excellent anti-scouring properties has been realized, which reduces the cost and increases the added value of lithium slag.

CN118754577APending Publication Date: 2024-10-11TONGJI UNIV

Patent Information

Application Number
CN202410838130.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing scour protection methods for offshore platform buildings are costly and pollute the environment, and lithium slag resources have not been effectively utilized. Lithium slag storage problems are serious, and existing anti-scouring curing agents have poor adaptability, which affects the safe operation of offshore platforms.

Method used

Modified lithium slag powder is used to form a multi-component composite gelling system with Portland cement and sulfoaluminate cement to prepare an offshore wind turbine foundation scour protection sludge curing agent. The porosity and activity are increased by calcining the lithium slag, combined with non-ionic Type polyacrylamide and xanthan gum are used as salt-resistant tackifiers to improve the viscosity and stability of the curing agent, and are used in seawater to form solidified soil with superior erosion resistance.

Benefits of technology

A marine sludge solidifier with high strength, rapid solidification, and excellent anti-scouring properties has been realized, which reduces the problem of lithium slag storage, increases the added value of lithium slag, reduces construction costs, and maintains stability and adaptability in seawater environments. powerful.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754577A_ABST
    Figure CN118754577A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, and relates to a lithium slag-doped offshore wind turbine foundation erosion protection sludge curing agent and preparation and application thereof, and the lithium slag-doped offshore wind turbine foundation erosion protection sludge curing agent comprises the following components: 30-60 parts of Portland cement, 10-40 parts of rapid hardening cement, 20-50 parts of modified lithium slag powder, 5-10 parts of a pH regulator, 0.2-2.0 parts of a salt-tolerant tackifier, and 1-2 parts of a dispersant. Compared with the prior art, the prepared ocean anti-scouring solidified soil is fast in underwater solidification, high in strength, not dispersed underwater in the construction process and good in anti-scouring effect, and the solidified soil can achieve self-leveling at the seabed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, and in particular to a lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent and a preparation and application thereof. Background Art

[0002] The existing supporting structures of offshore platform buildings are mainly pile foundations. The pile foundations are deep in the seabed mud. Under the influence of complex waves and currents, scouring is becoming increasingly serious, posing a hidden danger to the safe operation of offshore platforms. Nowadays, the common scouring protection method is mainly stone throwing, which can easily cause unevenness on the seabed, further increasing the probability of scouring. Although grouting underwater concrete has high strength, it consumes a lot of cement, sand and gravel and other resources, and the cost is high. On the other hand, marine silt dredging is a necessary way to solve the problem of safe navigation of ships and the construction of port and waterway infrastructure. The annual dredging output of marine silt is as high as hundreds of millions of tons, and the consolidation speed is slow, the bearing capacity is small, and a large amount of land yard is required. Silt resources are not effectively utilized.

[0003] Lithium slag is an industrial waste residue produced in the process of producing lithium carbonate and other lithium salts by sulfuric acid method from spodumene ore. 8-10 tons of lithium slag are discharged for every ton of lithium carbonate produced. In recent years, with the vigorous development of new energy batteries, the continuous expansion of the application fields of lithium salts such as lithium carbonate and lithium hydroxide and the rapid growth of market demand, the requirements for lithium extraction efficiency from lithium ore are also increasing. In recent years, the stockpile of lithium slag in my country has increased dramatically, and the SO3 content of discharged lithium slag is also higher than before. At present, most of the discharged lithium slag is treated by open-air stacking or deep pit landfill, which occupies the site and pollutes the environment, and wastes lithium slag resources. Therefore, how to use lithium slag in large amounts and with high added value is an urgent problem to be solved.

[0004] Chinese patent application CN111995339A discloses an anti-scour solidified soil for an offshore platform and its preparation method. The curing agent in the patent is mainly composed of cement, lime, mineral powder, cellulose and water reducer. The silt solidified soil prepared with the curing agent has low compressive strength and limited anti-scour ability. In addition, since the curing agent is mixed with anionic surfactants such as cellulose ether and naphthalene water reducer, a large amount of foam is generated during the stirring process. The foam floats on the sea surface with the waves and pollutes the marine environment. The anti-scour curing agents commonly used in current projects have poor adaptability to soil, and the influence of seawater on cementitious materials and soil has not been considered, resulting in poor working performance and mechanical properties of the solidified soil. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and to provide a lithium-doped offshore wind turbine foundation scour protection silt solidifier and its preparation and application. The silt solidifier of the present invention has the advantages of high strength, good pumping performance, excellent scour resistance, good curing effect, and no foam. It also makes full use of the porous and sulfur-rich characteristics of lithium slag, proposes a new solution to the storage problem of lithium slag, and has good environmental and economic benefits.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent, comprising the following components in parts by weight:

[0008]

[0009] A method for preparing a lithium slag-doped offshore wind turbine foundation scour protection sludge curing agent comprises the following steps: mixing silicate cement, rapid hardening cement, modified lithium slag powder, pH regulator, dispersant and salt-resistant thickener according to mass ratio and then dry-mixing to prepare the curing agent.

[0010] Furthermore, the preparation method of the modified lithium slag powder comprises:

[0011] The high sulfur lithium slag powder is calcined, and after calcination, the sample is ground to make its nitrogen adsorption specific surface area 7000-12000m 2 / kg to obtain modified lithium slag powder.

[0012] Furthermore, the calcination temperature is 500-700° C., and the holding time is 25-30 minutes.

[0013] Furthermore, the pH regulator is one or more of NaOH, sodium carbonate or sodium sulfate.

[0014] Furthermore, the salt-resistant thickener is prepared from non-ionic polyacrylamide and xanthan gum in a mass ratio of (10-40): (60-90), and the molecular weight of the non-ionic polyacrylamide is 8 million to 16 million.

[0015] Furthermore, the dispersant is a naphthalene-based powder water reducer.

[0016] Furthermore, the silicate cement is PI52.5 or PII525, and the rapid hardening cement is 42.5 sulphoaluminate cement.

[0017] An application of a lithium-doped slag offshore wind turbine foundation scouring protection sludge solidifying agent, wherein the lithium-doped slag offshore wind turbine foundation scouring protection sludge solidifying agent is used to solidify the protective sludge, and the application method thereof comprises:

[0018] S1: Take the seabed mud, sieve it, add seawater, and stir it evenly to form mud;

[0019] S2: Add 8-15wt% of a curing agent into the mud and stir evenly to obtain scour protection silt solidified soil;

[0020] S3: Pump the scour protection silt solidification soil to the root of the offshore platform pile foundation, solidify it into shape, and form a scour protection circle after hardening.

[0021] Furthermore, in step S1, seawater is added to control the water content of the sludge to 70-100%.

[0022] The invention utilizes the porous characteristics of lithium slag, the presence of anhydrous gypsum and a large amount of active silicon-aluminum compounds in the minerals after calcination, and combines the calcined lithium slag with silicate cement and sulphoaluminate cement to form a multi-component composite gelling system, and then adds slag powder, pH regulator, dispersant and salt-resistant viscosity enhancer to prepare the system.

[0023] Since lithium slag contains not only active SiO2 and Al2O3, but also nearly 20-45% dihydrate gypsum, by scientifically setting the calcination system, on the one hand, the dihydrate gypsum in the lithium slag can be converted into anhydrous gypsum, and on the other hand, the volcanic ash activity of the lithium slag can be improved. At the same time, the lithium slag produced by the spodumene sulfuric acid leaching and smelting process has a porous structure. After calcination, the porosity of the lithium slag is further increased, which increases the adsorption of free water.

[0024] The composite gelling system formed by the calcined lithium slag, silicate cement and sulphoaluminate in the present invention, silicate cement, sulphoaluminate and anhydrous gypsum in the composite gelling system can undergo hydration reaction at an early stage to generate a large amount of hydraulic CSH and AFt, thereby ensuring the mechanical properties of the early solidified soil and providing a mechanical framework for the subsequent strength growth of the solidified soil. With the increase of age, silicate cement and sulphoaluminate cement are further hydrated, while promoting the secondary hydration of silicon and aluminum in the lithium slag, thereby ensuring the later mechanical properties of the solidified soil. After the calcined lithium slag is added, the viscosity of the solidified soil can be improved due to the porous water absorption characteristics of the structure, thereby improving the stability of the solidified soil.

[0025] The pH regulator in the present invention can, on the one hand, increase the pH value of the slurry and improve the dispersibility of the sludge through the principle of charge repulsion. On the other hand, the increase in pH can stimulate the mineral powder and promote the cement hydration reaction, thereby improving the early mechanical properties of the composite cementitious system.

[0026] The salt-resistant thickener of the present invention adopts a composite combination of non-ionic polyacrylamide and xanthan gum. + and Ca 2+Ionic and non-ionic polyacrylamide and xanthan gum not only have good viscosity-increasing properties, but also have excellent salt resistance, which ensures the underwater non-dispersion and stability of the solidified soil and improves its adaptability to different seawaters.

[0027] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0028] (1) The present invention prepares marine anti-scour solidified soil, which has fast underwater solidification and high strength. It does not disperse underwater during construction and has good anti-scour effect. Moreover, the solidified soil can achieve self-leveling on the seabed.

[0029] (2) The present invention has excellent adaptability to various types of sludge and is highly resistant to salt water environments.

[0030] (3) A large amount of lithium slag solid waste is utilized, which increases the added value of lithium slag and reduces product production and construction costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the X-ray powder polycrystalline diffractometer (XRD) spectrum of the modified lithium slag used in Example 1. DETAILED DESCRIPTION

[0032] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0033] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0034] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.

[0035] In the following examples, the seabed sludge used in the test was taken from a sea area in Dalian City, and the physical property indicators of the sludge are shown in Table 1.

[0036] The moisture content of the silt reaches 70.1% and the liquid limit reaches 62.8%. According to the soil classification method, the test silt belongs to high-moisture-content and high-liquid-limit clay.

[0037] Table 1 Performance parameters of seabed silt

[0038]

[0039] In the following embodiments, cement is Jiangxi Wannianqing PII525 cement, sulphoaluminate cement is purchased from Tangshan Polar Bear Cement, modified lithium slag powder is purchased from Jiangxi Ganfeng Lithium Co., Ltd., pH regulator and salt-resistant viscosity enhancer are purchased from Xiamen Zhengxingxing Trading Co., Ltd., dispersant is purchased from Zhejiang Tongwei Building Materials Co., Ltd., and sulfur-rich lithium slag is purchased from Jiangxi Ganfeng Lithium Co., Ltd.

[0040] Example 1

[0041] The present embodiment provides a marine sludge solidifying agent and its preparation method. 30 parts of silicate cement, 30 parts of 42.5 sulphoaluminate cement, 35 parts of modified lithium slag powder, 5 parts of pH regulator, 0.8 parts of salt-resistant thickener, and 1.9 parts of dispersant are weighed by mass, and the mixture is mechanically mixed in a mixer and dry-mixed for 5 minutes to obtain the marine sludge solidifying agent of the present embodiment.

[0042] The modified lithium slag powder is produced by calcining sulfur-rich lithium slag at about 600°C. The high-sulfur lithium slag powder is calcined so that the sample is heated from room temperature to 600°C within 20 minutes, and the heat preservation time is 30 minutes. After calcination, the sample is taken out and rapidly cooled in the air, and the calcined sample is ground for 60 minutes to make its nitrogen adsorption specific surface area 7000-12000m 2 / kg, and modified lithium slag powder is obtained.

[0043] Among them, the mass percentage of SO3 in the high-sulfur lithium slag is higher than 15%.

[0044] The salt-resistant thickener is obtained by mixing xanthan gum and nonionic polyacrylamide in a mass ratio of 50:50. Figure 1 This is the X-ray powder polycrystalline diffractometer (XRD) spectrum of the modified lithium slag in Example 1. It can be seen from the figure that the amorphous part in the modified lithium slag is significantly increased, making the lithium slag more active.

[0045] Performance testing method:

[0046] S1: Take 500 kg of seabed mud, sieve to remove large-sized stones, weeds and garbage, add seawater to adjust the moisture content of the sea mud to 85%, and stir evenly to form mud;

[0047] S2: Add 160 kg of solidifying agent to every cubic meter of marine silt and stir evenly to obtain scour protection silt solidified soil. Specific indicators are shown in Table 2.

[0048] Example 2

[0049] The present embodiment provides a marine sludge solidifying agent and its preparation method. 20 parts of silicate cement, 40 parts of 42.5 sulphoaluminate cement, 37 parts of modified lithium slag powder, 3 parts of pH regulator, 0.6 parts of salt-resistant thickener, and 2 parts of dispersant are weighed by mass, and the mixture is mechanically mixed in a mixer and dry-mixed for 5 minutes to obtain the marine sludge solidifying agent of the present embodiment.

[0050] Among them, the modified lithium slag powder is produced by calcining sulfur-rich lithium slag at about 650°C.

[0051] The salt-resistant thickener is xanthan gum and non-ionic polyacrylamide in a mass ratio of 30:70.

[0052] Performance testing method:

[0053] Take 500 kg of seabed mud, sieve to remove large-sized stones, weeds and garbage, add seawater to adjust the moisture content of the sea mud to 90%, and stir evenly to form mud;

[0054] S2: Add 160 kg of solidifying agent to every cubic meter of marine silt and stir evenly to obtain scour protection silt solidified soil. Specific indicators are shown in Table 2.

[0055] Example 3

[0056] The present embodiment provides a marine sludge solidifying agent and its preparation method. 40 parts of silicate cement, 20 parts of 42.5 sulphoaluminate cement, 37 parts of modified lithium slag powder, 3 parts of pH regulator, 0.5 parts of salt-resistant thickener, and 2.2 parts of dispersant are weighed by mass, and the mixture is mechanically mixed in a mixer and dry-mixed for 5 minutes to obtain the marine sludge solidifying agent of the present embodiment.

[0057] Among them, the modified lithium slag powder is produced by calcining sulfur-rich lithium slag at about 600°C.

[0058] The mass ratio of the salt-resistant thickener, xanthan gum and non-ionic polyacrylamide, is 75:25.

[0059] Performance testing method:

[0060] Take 500 kg of seabed mud, sieve to remove large-sized stones, weeds and garbage, add seawater to adjust the water content of the sea mud to 85%, and stir evenly to form mud;

[0061] S2: Add 160 kg of solidifying agent to every cubic meter of marine silt and stir evenly to obtain scour protection silt solidified soil. Specific indicators are shown in Table 2.

[0062] Comparative Example 1

[0063] A marine sludge solidifying agent is prepared by weighing 100 parts of silicate cement and 2 parts of dispersant by weight.

[0064] According to this ratio, the solidified soil is prepared. When the water content of the marine silt is 95%, 160 kg of the solidifying agent is added to each cubic meter of the marine silt, and the solidified soil is obtained by proper stirring. Specific indicators are shown in Table 2.

[0065] Comparative Example 2

[0066] A marine sludge solidifying agent is prepared by weighing, by mass, 50 parts of ordinary Portland cement, 50 parts of sulphoaluminate cement and 2.2 parts of a dispersant.

[0067] According to this ratio, the solidified soil is prepared. When the water content of the marine silt is 100%, 180 kg of the solidifying agent is added to each cubic meter of the marine silt, and the solidified soil is obtained by proper stirring. Specific indicators are shown in Table 2.

[0068] Table 2 Curing performance of Examples 1-3 and Comparative Examples 1-2

[0069]

[0070] The initial slump and 30-minute slump refer to the standard GB / T 50080-2002 "Standard for test methods for properties of ordinary concrete mixtures", and the other indicators refer to CJ / T486-2015 "Soil Stabilizing Admixtures".

[0071] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent, characterized in that: According to parts by weight, it comprises the following components:

2. A method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent as claimed in claim 1, characterized in that: The method comprises the following steps: mixing silicate cement, quick-hardening cement, modified lithium slag powder, pH regulator, dispersant and salt-resistant thickener according to mass ratio and then dry-mixing to prepare the curing agent.

3. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 2, characterized in that: The preparation method of the modified lithium slag powder comprises: The high sulfur lithium slag powder is calcined, and after calcination, the sample is ground to make its nitrogen adsorption specific surface area 7000-12000m 2 / kg to obtain modified lithium slag powder.

4. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 3, characterized in that: The calcination temperature is 500-700° C., and the heat preservation time is 25-30 minutes.

5. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 2, characterized in that: The pH regulator is one or more of NaOH, sodium carbonate or sodium sulfate.

6. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 2, characterized in that: The salt-resistant thickener is prepared from nonionic polyacrylamide and xanthan gum in a mass ratio of (10-40): (60-90), and the molecular weight of the nonionic polyacrylamide is 8 million to 16 million.

7. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 2, characterized in that: The dispersant is a naphthalene-based powder water reducer.

8. The method for preparing the lithium slag-doped offshore wind turbine foundation scour protection sludge solidifying agent according to claim 2, characterized in that: The silicate cement is PI52.5 or PII525, and the rapid hardening cement is 42.5 sulphoaluminate cement.

9. An application of the lithium-doped slag scour protection sludge solidifying agent for offshore wind turbine foundation as claimed in claim 1, characterized in that: The lithium slag-doped offshore wind turbine foundation scouring protection sludge solidifying agent is used to solidify the protective sludge, and its application method includes: S1: Take the seabed mud, sieve it, add seawater, and stir it evenly to form mud; S2: Add 8-15wt% of a curing agent into the mud and stir evenly to obtain scour protection silt solidified soil; S3: Pump the scour protection silt solidification soil to the root of the offshore platform pile foundation, solidify it into shape, and form a scour protection circle after hardening.

10. The use of the lithium-doped slag sludge solidifying agent for offshore wind turbine foundation scour protection according to claim 9, characterized in that: In step S1, seawater is added to control the water content of the sludge to 70-100%.

Citation Information

Patent Citations

  • Salinized soil curing agent prepared from industrial waste slag

    CN102002366A

  • Super early strong cement base underwater non-dispersible repairing material and preparation method

    CN110183193A

  • Anti-scouring solidified soil for ocean platform and preparation method thereof

    CN111995339A

  • Self-flowing cohesive soil and preparation method thereof

    CN114890722A

  • High-water-content anti-scouring sludge curing grouting material as well as preparation method and application thereof

    CN115849775A

Cited By

  • Underwater anti-scouring curing agent based on all-solid waste salt-alkali synergistic excitation and preparation method thereof

    CN121872745A