NTC (Negative Temperature Coefficient) thermal sensitive ceramic material with low resistance value and high breaking strength and preparation method of NTC thermal sensitive ceramic material
By adding MgO, Bi2O3 and CaO to NTC thermosensitive ceramic materials and adjusting the element composition and process flow, the problems of low resistivity stability and low flexural strength of existing NTC thermosensitive ceramic materials have been solved, achieving high stability and high Prepared from ceramic materials with high flexural strength, suitable for high-performance thermal components.
Patent Information
- Application Number
- CN202410749296.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-12
AI Technical Summary
Existing NTC thermosensitive ceramic materials have poor resistivity stability at high temperatures, are prone to price changes, and have low flexural strength, which limits their application in high-end fields.
By adding MgO, Bi2O3 and CaO to the NTC thermosensitive ceramic material, the element composition is adjusted to CuxNi0.60Mn2.40-x-y-z-wMgyBizCawO4, and is prepared using ball milling, dry pressing and sintering processes to form a product with low resistance and high flexural strength. spinel structure ceramic material.
It significantly improves the resistivity stability and flexural strength of the material, ensuring the high stability, reliability and long life of thermal components, and is suitable for the industrial production of high-performance thermal components.
Smart Images

Figure CN118754640A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermosensitive ceramic materials, and in particular to an NTC thermosensitive ceramic material with low resistance and high flexural strength and a preparation method thereof. Background Art
[0002] NTC (Negative Temperature Coefficient) thermistor ceramic materials are generally composed of two or more transition metal oxides such as Mn, Co, Ni, Al, Fe, Cu, etc., and have a spinel structure when synthesized at high temperature. It is a characteristic material with a resistance that decreases with increasing temperature. This type of ceramic material has many advantages such as fast temperature response, high power, strong surge current suppression ability, long life, high reliability, and small size. It is widely used in surge current suppression, temperature measurement, temperature compensation, etc.
[0003] NTC thermistor ceramic materials are usually composed of transition metals with AB 2 O 4 Spinel structured composite oxides, for spinel structured NTC thermistor materials, all use the addition of Cu elements to effectively reduce the resistivity and B value of NTC thermistor materials, especially materials with extremely low resistivity and high B. However, the stability of the Cu element-containing system is poor. Due to the easy valence change of the Cu element, it inevitably brings about aging problems and the low strength of low-resistance ceramic materials and easy breakage during use. This greatly restricts the application of low-resistance NTC thermistor ceramic resistors in high-end fields such as high-requirement switching power supplies, precision temperature control and temperature measurement.
[0004] Therefore, how to prepare an NTC thermistor ceramic material with both good flexural strength and low resistivity is crucial for the thermistor component industry. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and provide an NTC thermistor ceramic material with low resistance and high flexural strength and a preparation method thereof. The NTC thermistor ceramic material of the present invention has the characteristics of extremely low ρ, good flexural strength, and greatly improved stability of ρ value and B value. The thermistor components prepared by using the material have the advantages of high stability, high reliability, long life, etc., and have important practical value for the industrial production of high-performance thermistor components.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] In a first aspect, the present invention provides an NTC thermistor ceramic material with low resistance and high flexural strength, wherein the element composition of the NTC thermistor ceramic material is Cu x Ni 0.60 Mn2.40-x-y-z-w Mg y Bi z Ca w O 4 , where 0 <x≤0.9,0<y≤0.35,0<z≤0.15,0<w≤0.3。
[0008] The present invention adds MgO, Bi and 2 O 3 and CaO to prepare a spinel structure NTC thermistor ceramic material with low resistivity and good flexural strength.
[0009] Preferably, 0.3≤x≤0.8, 0.10≤y≤0.35, 0.03≤z≤0.15, and 0.03≤w≤0.30.
[0010] Preferably, the NTC thermistor ceramic material is a Cu-Ni-Mn ternary system with MgO, Bi 2 O 3 And CaO.
[0011] In a second aspect, the present invention further provides a method for preparing an NTC thermistor ceramic material, comprising the following steps:
[0012] (1) Mn 3 O 4 、NiO、CuO、MgO、Bi 2 O 3 The six oxides of Cu, CaO are weighed according to the following molar composition ratio: x Ni 0.60 Mn 2.40-x-y-z-w Mg y Bi z Ca w O 4 , where 0 <x≤0.9,0<y≤0.35,0<z≤0.15,0<w≤0.3;
[0013] (2) placing the weighed material, zirconium balls, and deionized water in step (1) into a ball mill for ball milling, and then drying the milled slurry in an oven, and passing the dried material through a sieve;
[0014] (3) granulating the powder obtained in step (2);
[0015] (4) dry-pressing the powder in step (3) to obtain a ceramic body after debinding and high-temperature sintering;
[0016] (5) The ceramic body obtained in step (4) is polished and coated with silver paste on both sides as electrodes to obtain an NTC thermistor ceramic material.
[0017] Preferably, the ball milling speed in step (2) is 300-500 rpm, and the ball milling time is 3-6 hours.
[0018] Preferably, in step (2), the mass ratio of the material, zirconium balls and deionized water is 1:(3-5):1.5.
[0019] Preferably, in step (2), the slurry after ball milling is poured out and dried at 80-95° C. for 18-25 hours.
[0020] Preferably, in step (2), the dried material is passed through a 100-120 mesh sieve.
[0021] Preferably, in step (4), the sintering temperature is 1000-1200° C. and the sintering time is 2-3 hours.
[0022] Preferably, the silver calcining conditions in step (5) are as follows: the room temperature is raised to 100-120° C. over 25-30 minutes, then kept warm for 10-12 minutes, then raised to 320-350° C. over 55-60 minutes, then kept warm for 8-10 minutes, then raised to 650-660° C. over 55-60 minutes, then kept warm for 30-35 minutes.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention adopts manganese nickel copper and MgO, Bi 2 O 3 , CaO composite material system, by changing the values of x, y, z, and w, it is possible to adjust the material B value while obtaining extremely low resistivity, thereby ensuring good flexural strength of the ceramic body, and under long-term aging conditions at 150°C, the change rates of ρ and B values are both less than 1.3%; compared with existing NTC thermistor ceramic materials, the material system provided by the present invention has the characteristics of extremely low ρ, good flexural strength, and greatly improved stability of ρ and B values. The thermistor components prepared using the material have the advantages of high stability, high reliability, and long life, and have important practical value for the industrial production of high-performance thermistor components. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a preparation flow chart of the NTC thermistor ceramic material of the present invention. DETAILED DESCRIPTION
[0026] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the protection scope and implementation methods of the present invention are not limited thereto.
[0027] Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0028] The raw materials and specifications used in the examples of the present invention are shown in Table 1.
[0029] Table 1
[0030] raw material Molecular weight purity <![CDATA[Manganese tetraoxide (Mn 3 O 4 )]]> 228.82 99.6% Nickel Oxide (NiO) 74.70 99.6% Copper Oxide (CuO) 79.55 99.6% Magnesium oxide (MgO) 40.30 99.6% <![CDATA[Bismuth(III) oxide (Bi 2 O 3 )]]> 465.96 99.6% Calcium oxide (CaO) 56.08 99.6%
[0031] Example 1
[0032] A method for preparing an NTC thermistor ceramic material comprises the following steps:
[0033] (1) Batching, ball milling and drying
[0034] According to Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Bi 0.09 Ca 0.10 O 4 The ingredients are mixed in proportion; the weighed raw materials, zirconium balls and deionized water are put into a ball mill according to a weight ratio of 1:3:1.5, and ball milled for 6 hours at 300 rpm using a planetary ball mill; after ball milling, the slurry is poured out and placed in an oven for drying at a constant temperature of 90°C for 20 hours, and the dried material is passed through a 100-mesh stainless steel sieve.
[0035] (2) Granulation
[0036] A 6 wt.% polyvinyl alcohol (PVA) aqueous solution binder was added to the sieved powder, and the mixture was fully ground and mixed in a mortar for granulation. The mixture was then passed through 60-mesh and 100-mesh sieves to select the granules in the middle layer.
[0037] (3) Dry pressing
[0038] The particles prepared in step (2) were placed in a steel mold and dry pressed into cylindrical green sheets of Φ16.00 mm×2.20 mm on a hydraulic press at a pressure of 400 MPa·m -2 (Pressure converted based on the area of the pressure column).
[0039] (4) Debinding and sintering process
[0040] The green body formed in step (3) is placed in a box-type resistance furnace, heated from room temperature to 350°C over 232 minutes, kept warm for 2 hours for debinding treatment, then heated to 1180°C over 5 hours and kept warm for 3 hours, cooled in the furnace, and a dense ceramic body is prepared.
[0041] (5) Silver coating
[0042] The ceramic body sintered in step (4) is polished and coated with silver paste on both sides as electrodes. The silver sintering system is as follows: the temperature is raised from room temperature (25°C) to 120°C for 30 minutes, kept warm for 10 minutes, then raised to 350°C for 60 minutes and kept warm for 10 minutes, then raised to 650°C for 60 minutes, kept warm for 30 minutes, and cooled in the furnace to prepare the NTC thermistor ceramic material.
[0043] (6) Testing
[0044] ρ25 test: According to the R25 resistance value of the chip after silver coating and the size of the ceramic piece, the resistivity ρ of the ceramic piece is calculated; flexural strength test: The sintered ceramic piece is tested for its strength using the Shanghai Qingji QJWE-2000 flexural strength tester; B25 / 85 test: The resistance at 25℃ and 85℃ is tested respectively, and the B value is calculated; Aging treatment is performed on the test sample: Keep it at 150℃ for 50 hours, and test the resistance at 25℃ and 85℃ after aging respectively. The B value after aging is calculated according to formula (a): B=1779.7×ln(R25 / R85)(a).
[0045] The test performance of the NTC thermistor ceramic material obtained in Example 1 is shown in Table 2.
[0046] Table 2Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Bi 0.09 Ca 0.10 O 4 Properties of ceramic materials
[0047]
[0048]
[0049] From the results in Table 2, we can see that Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Bi 0.09 Ca 0.10 O 4 The B value of the three samples of thermistor ceramic materials is maintained at around 2630K, and the resistivity is about 3.3Ω.cm. After aging at 150℃ for 50h, the change rate of B value and resistivity is much less than 1.3%, and the flexural strength of the ceramic body is about 250N.
[0050] Example 2
[0051] A method for preparing an NTC thermistor ceramic material comprises the following steps:
[0052] (1) Batching, ball milling and drying
[0053] According to Cu 0.4 Ni 0.60 Mn 1.20 Mg 0.35 Bi 0.15 Ca 0.3 O 4 The weighed raw materials, zirconium balls and deionized water are placed in a ball mill according to a weight ratio of 1:3:1, and the ball mill is used for 3 hours at a speed of 500 rpm in a planetary ball mill; after ball milling, the slurry is poured out and placed in an oven at a constant temperature of 80°C for 25 hours to dry, and the dried material is passed through a 100-mesh stainless steel sieve.
[0054] (2) Granulation
[0055] A 6 wt.% polyvinyl alcohol (PVA) aqueous solution binder was added to the sieved powder, and the mixture was fully ground and mixed in a mortar to form granules. The granules were then passed through 60 and 100 mesh sieves to select the granules in the middle layer.
[0056] (3) Dry pressing
[0057] The particles prepared in step (2) were placed in a steel mold and dry pressed into cylindrical green sheets of Φ16.00 mm×2.20 mm on a hydraulic press at a pressure of 400 MPa·m -2 (Pressure converted based on the area of the pressure column).
[0058] (4) Debinding and sintering process
[0059] The green body formed in step (3) is placed in a box-type resistance furnace, heated from room temperature to 350°C over 232 minutes, kept warm for 2 hours for debinding treatment, then heated to 1180°C over 5 hours and kept warm for 3 hours, cooled in the furnace, and a dense ceramic body is prepared.
[0060] (5) Silver coating
[0061] The ceramic body sintered in step (4) is polished and coated with silver paste on both sides to serve as electrodes. The silver sintering system is as follows: the temperature is raised from room temperature (25°C) to 120°C over 30 minutes, kept warm for 10 minutes, then raised to 350°C over 60 minutes and kept warm for 10 minutes, then raised to 660°C over 60 minutes, kept warm for 30 minutes, and cooled in the furnace to prepare the NTC thermistor ceramic material.
[0062] (6) Testing
[0063] The resistance at 25°C and 85°C was tested respectively, and the room temperature resistivity ρ, B value and porcelain flexural strength were calculated according to the method of Example 1; the test samples were subjected to aging treatment: 150°C for 50 hours.
[0064] The test performance of the NTC thermistor ceramic material obtained in Example 2 is shown in Table 3.
[0065] Table 3Cu 0.4 Ni 0.60 Mn 1.20 Mg 0.35 Bi 0.15 Ca 0.3 O 4 Properties of ceramic materials
[0066]
[0067] From the results in Table 3, we can see that Cu 0.4 Ni 0.60 Mn 1.20 Mg 0.35 Bi 0.15 Ca 0.3 O 4 The B value of the three samples of ceramic materials was maintained at around 3000K, and the resistivity was about 51Ω·cm. After aging at 150℃ for 50h, the change rate of B value and resistance R value was much less than 1.3%, and the flexural strength of the ceramic body was about 525N.
[0068] Comparative Example 1
[0069] A method for preparing an NTC thermistor ceramic material comprises the following steps:
[0070] (1) Batching, ball milling and drying
[0071] According to Cu 1.0 Ni 0.60 Mn 1.31 Mg 0.05 Bi 0.02 Ca 0.02 O 4 The weighed raw materials, zirconium balls and deionized water were put into a ball mill according to a weight ratio of 1:3:1.2, and the slurry was poured out at a speed of 500 rpm for 3 hours in a planetary ball mill; the slurry was placed in an oven at a constant temperature of 110°C for 18 hours for drying, and the dried material was passed through a 100-mesh stainless steel sieve.
[0072] (2) Granulation
[0073] A 6 wt.% polyvinyl alcohol (PVA) aqueous solution binder was added to the sieved powder, and the mixture was fully ground and mixed in a mortar to form granules. The granules were then passed through 60 and 100 mesh sieves to select the granules in the middle layer.
[0074] (3) Dry pressing
[0075] The particles prepared in step (2) are placed in a steel mold and dry pressed on a hydraulic press into cylindrical green sheets of Φ16.00 mm×2.20 mm at a pressure of 400 MPa·m-2 (pressure converted based on the area of the pressure column).
[0076] (4) Debinding and sintering process
[0077] The green body formed in step (3) is placed in a box-type resistance furnace, heated from room temperature to 350°C over 232 minutes, kept warm for 2 hours for debinding treatment, then heated to 1200°C over 5 hours and kept warm for 3 hours, cooled in the furnace, and a dense ceramic body is prepared.
[0078] (5) Silver coating
[0079] The ceramic body sintered in step (5) is polished and coated with silver paste on both sides to serve as electrodes. The silver sintering system is as follows: the temperature is raised from room temperature (25±5°C) to 120°C for 30 minutes, then kept warm for 10 minutes, then raised to 350°C for 60 minutes, then kept warm for 10 minutes, then raised to 650°C for 60 minutes, kept warm for 30 minutes, and cooled in the furnace to prepare the NTC thermistor ceramic material.
[0080] (6) Testing
[0081] The resistance at 25°C and 85°C was tested respectively, and the room temperature resistivity ρ, B value and porcelain flexural strength were calculated according to the method of Example 1; the test samples were subjected to aging treatment: 150°C for 50 hours.
[0082] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 1 is shown in Table 4.
[0083] Table 4Cu 1.0 Ni 0.60 Mn 1.31 Mg 0.05 Bi 0.02 Ca 0.02 O 4 Properties of ceramic materials
[0084]
[0085] From the results in Table 4, we can see that Cu 1.0 Ni 0.60 Mn 1.31 Mg 0.05 Bi 0.02 Ca 0.02 O 4The B value of the three samples of ceramic material was maintained at about 3500K, and the resistivity was about 95Ω·cm. After aging at 150°C for 50h, the change rate of B value and resistance R value was less than 1.3% as a whole, but it was deteriorated compared with the results of Example 1 and Example 2, and the flexural strength of the ceramic body was less than 90N.
[0086] Comparative Example 2
[0087] A method for preparing an NTC thermistor ceramic material, which is different from that of Example 1 in that the element composition of the NTC thermistor ceramic material in step (1) is Cu 0.7 Ni 0.60 Mn 1.01 Mg 0.5 Bi 0.09 Ca 0.10 O 4 , wherein x=0.7, y=0.5, z=0.09, w=0.10, and the others are the same as those in Example 1.
[0088] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 2 is shown in Table 5.
[0089] Table 5Cu 0.7 Ni 0.60 Mn 1.01 Mg 0.5 Bi 0.09 Ca 0.10 O 4 Properties of ceramic materials
[0090]
[0091] From the results in Table 5, we can see that Cu 0.7 Ni 0.60 Mn 1.01 Mg 0.5 Bi 0.09 Ca 0.10 O 4 The B value of the three samples of ceramic material was maintained at about 3600K, and the resistivity was about 150Ω·cm. After aging at 150℃ for 50h, the change rates of B value and resistance R value were both greater than 1.49%, and the flexural strength of the ceramic body was about 73N. It can be seen that its resistivity is much greater than the low resistance range of 3.3 to 51Ω·cm of Example 1 and Example 2, and the flexural strength of the ceramic body and its B value and resistance R value change rate are all worse than the results of Example 1 and Example 2.
[0092] Comparative Example 3
[0093] A method for preparing an NTC thermistor ceramic material, which is different from that of Example 1 in that the element composition of the NTC thermistor ceramic material in step (1) is Cu 0.7Ni 0.60 Mn 1.15 Mg 0.15 Bi 0.3 Ca 0.10 O 4 , wherein x=0.7, y=0.15, z=0.3, w=0.10, and the others are the same as those in Example 1.
[0094] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 3 is shown in Table 6.
[0095] Table 6Cu 07 Ni 060 Mn 115 Mg 015 Bi 03 Ca 010 O 4 Properties of ceramic materials
[0096]
[0097]
[0098] From the results in Table 6, we can see that Cu 0.7 Ni 0.60 Mn 1.15 Mg 0.15 Bi 0.3 Ca 0.10 O 4 The B value of the three samples of ceramic material was maintained at about 3800K, and the resistivity was about 180Ω·cm. After aging at 150°C for 50h, the change rates of B value and resistance R value were both greater than 1.58%, and the flexural strength of the ceramic body was about 108N. It can be seen that its resistivity is much greater than the low resistance range of 3.3 to 51Ω·cm of Example 1 and Example 2, and the flexural strength of the ceramic body and its B value and resistance R value change rate are all worse than the results of Example 1 and Example 2.
[0099] Comparative Example 4
[0100] A method for preparing an NTC thermistor ceramic material, which is different from that of Example 1 in that the element composition of the NTC thermistor ceramic material in step (1) is Cu 0.7 Ni 0.60 Mn 0.96. Mg 0.15 Bi 0.09 Ca 0.50 O 4 , wherein x=0.7, y=0.15, z=0.09, w=0.50, and the others are the same as those in Example 1.
[0101] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 4 is shown in Table 7.
[0102] Table 7Cu 0.7 Ni 0.60 Mn 0.96. Mg 0.15 Bi 0.09 Ca 0.50 O 4 Properties of ceramic materials
[0103]
[0104] From the results in Table 7, we can see that Cu 0.7 Ni 0.60 Mn 0.96. Mg 0.15 Bi 0.09 Ca 0.50 O 4 The B value of the three samples of ceramic material was maintained at about 3200K, and the resistivity was about 80Ω·cm. After aging at 150°C for 50h, the change rates of B value and resistance R value were both greater than 1.38%, and the flexural strength of the porcelain body was about 63N. It can be seen that its resistivity is much greater than the low resistance range of 3.3 to 51Ω·cm of Example 1 and Example 2, and the flexural strength of the porcelain body and its B value and the change rate of resistance R value are all worse than the results of Example 1 and Example 2.
[0105] Comparative Example 5
[0106] A method for preparing an NTC thermistor ceramic material, which is different from that of Example 1 in that in step (1), an equimolar amount of TiO 2 Replace MgO, that is, the element composition of the NTC thermistor ceramic material is Cu 0.7 Ni 0.60 Mn 1.36 Ti 0.15 Bi 0.09 Ca 0.1 0 O 4 , wherein x=0.7, y=0.15, z=0.09, w=0.10, and the others are the same as those in Example 1.
[0107] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 5 is shown in Table 8.
[0108] Table 8Cu 0.7 Ni 0.60 Mn 1.36 Ti 0.15 Bi 0.09 Ca 0.10 O 4 Properties of ceramic materials
[0109]
[0110] From the results in Table 8, we can see that Cu 0.7 Ni 0.60 Mn 1.36 Ti 0.15 Bi 0.09 Ca 0.10 O 4 The B value of the three samples of ceramic material was maintained at about 3830K, and the resistivity was about 250Ω·cm. After aging at 150°C for 50h, the change rates of B value and resistance R value were both greater than 2.03%, and the flexural strength of the ceramic body was about 152N. It can be seen that its resistivity is much greater than the low resistance range of 3.3 to 51Ω·cm of Example 1 and Example 2, and the flexural strength of the ceramic body, its B value, and the change rates of resistance R value are nearly times worse than the results of Example 1 and Example 2.
[0111] Comparative Example 6
[0112] A method for preparing an NTC thermistor ceramic material, which is different from that of Example 1 in that in step (1), an equimolar amount of Nb 2 O 5 Replace Bi 2 O 3 , that is, the element composition of the NTC thermistor ceramic material is Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Nb 0.09 Ca 0.10 O 4 , wherein x=0.7, y=0.15, z=0.09, w=0.10, and the others are the same as those in Example 1.
[0113] The test performance of the NTC thermistor ceramic material obtained in Comparative Example 6 is shown in Table 9.
[0114] Table 9Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Nb 0.09 Ca 0.10 O 4 Properties of ceramic materials
[0115]
[0116]
[0117] From the results in Table 9, we can see that Cu 0.7 Ni 0.60 Mn 1.36 Mg 0.15 Nb 0.09 Ca0.10 O 4 The B value of the three samples of ceramic material was maintained at about 3500K, and the resistivity was about 200Ω·cm. After aging at 150°C for 50h, the change rates of B value and resistance R value were both greater than 1.96%, and the flexural strength of the porcelain body was about 95N. It can be seen that its resistivity is much greater than the low resistance range of 3.3 to 51Ω·cm of Example 1 and Example 2, and the flexural strength of the porcelain body and its B value and the change rate of resistance R value are all several times worse than the results of Example 1 and Example 2.
[0118] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. An NTC thermistor ceramic material with low resistance and high flexural strength, characterized in that: The element composition of the NTC thermistor ceramic material is Cu x Ni 0.60 Mn 2.40-x-y-z-w Mg y Bi z Ca w O4, where 0 <x≤0.9,0<y≤0.35,0<z≤0.15,0<w≤0.3。 2. The NTC thermistor ceramic material according to claim 1, characterized in that: 0.3≤x≤0.8, 0.10≤y≤0.35, 0.03≤z≤0.15, 0.03≤w≤0.
30.
3. The NTC thermistor ceramic material according to claim 1, characterized in that: The NTC thermistor ceramic material is prepared by adding MgO, Bi2O3 and CaO to a Cu-Ni-Mn ternary system.
4. The method for preparing the NTC thermistor ceramic material according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Weigh six oxides, Mn3O4, NiO, CuO, MgO, Bi2O3, and CaO according to the following molar composition ratio: Cu x Ni 0.60 Mn 2.40-x-y-z-w Mg y Bi z Ca w O4, where 0 <x≤0.9,0<y≤0.35,0<z≤0.15,0<w≤0.3; (2) placing the weighed material, zirconium balls, and deionized water in step (1) into a ball mill for ball milling, and then drying the milled slurry in an oven, and passing the dried material through a sieve; (3) granulating the powder obtained in step (2); (4) dry-pressing the powder in step (3) to obtain a ceramic body after debinding and high-temperature sintering; (5) The ceramic body obtained in step (4) is polished and coated with silver paste on both sides as electrodes to obtain an NTC thermistor ceramic material.
5. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: The ball milling speed in step (2) is 300-500 rpm, and the ball milling time is 3-6 hours.
6. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: In the step (2), the mass ratio of the material, the zirconium balls and the deionized water is 1:(3-5):1.
5.
7. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: In the step (2), the slurry after ball milling is poured out and dried at 80-95° C. for 18-25 hours.
8. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: In the step (2), the dried material is passed through a 100-120 mesh sieve.
9. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: In the step (4), the sintering temperature is 1000-1200° C. and the sintering time is 2-3 hours.
10. The method for preparing the NTC thermistor ceramic material according to claim 4, characterized in that: The silver calcining conditions in step (5) are as follows: the room temperature is raised to 100-120° C. over 25-30 minutes, then kept warm for 10-12 minutes, then raised to 320-350° C. over 55-60 minutes, then kept warm for 8-10 minutes, then raised to 650-660° C. over 55-60 minutes, then kept warm for 30-35 minutes.
Citation Information
Patent Citations
High evenness negative temperature coefficient heat-sensitive resistance material and its preparation method
CN101127266A
High-resistivity / low-B value thermistor composition and method of producing the same
CN101492289A
Cobalt-free NTC ceramic and method for producing a cobalt-free NTC ceramic
CN102958866A
Thermal sensitive ceramic material with low resistivity, high B value and negative temperature coefficient and preparation method thereof
CN104193306A
NTC thermal sensitive ceramic material and preparation method thereof
CN111484314A