Preparation method of sweating structure porous ceramic based on digital light processing technology

The preparation of ceramic sweating structures through digital light processing technology solves the problems of stability and processing difficulty of metal sweating cooling at high temperatures, improves the high-temperature stability and mechanical properties of ceramic sweating structures, and meets the needs of high-temperature thermal protection in the aerospace field.

CN118754652APending Publication Date: 2024-10-11JIANGSU QIANDU ZHIZAO HI TECH CO LTD

Patent Information

Application Number
CN202410749620.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing metal sweating cooling structure cannot ensure stable operation for a long time under conditions of high temperature and high heat flux density. It is also difficult to process and cannot meet the high temperature thermal protection needs in the aerospace field.

Method used

Digital light processing technology is used to prepare ceramics as perspiration structural materials. Porous ceramics are manufactured through light-curing ceramic additive processes. Three-dimensional model slicing and light-curing printing technology are used to directionally control the pore size and flow channel distribution. The degreasing and sintering processes are combined to improve the high-temperature stability of the ceramics. and mechanical properties.

Benefits of technology

The high-temperature stability and mechanical properties of the ceramic sweating structure are improved, the service life is extended, the density and mechanical strength of the pore structure are improved, and the high-temperature thermal protection needs of the aerospace field are met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754652A_ABST
    Figure CN118754652A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of digital light processing 3D printing, and particularly relates to a sweating structure porous ceramic preparation method based on a digital light processing technology, which comprises the following steps: mixing at least two resin monomers to prepare a resin premixed solution; adding an auxiliary agent into the resin premixed liquid, and mixing to prepare the photosensitive resin; uniformly mixing photosensitive resin and ceramic powder to prepare porous ceramic slurry with a sweating structure; and setting corresponding photocuring printing conditions for printing, preparing a porous ceramic green body with the sweating structure, and degreasing and sintering to prepare the porous ceramic with the sweating structure. Printing groups with different thicknesses are arranged during printing, pore walls of pore structures formed through printing are continuously formed, pore diameter distribution and runner trend in sweating structures of the adjacent pore structures can be directionally controlled, the pore diameter specification is controlled according to requirements, and the printing efficiency is obviously improved; compared with the existing silicon carbide sweating structure porous ceramic manufactured by dry pressing, the silicon carbide sweating structure porous ceramic is denser and high in mechanical strength, and the service life of the sweating structure is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of digital light processing 3D printing, and in particular to a method for preparing porous ceramics with a sweating structure based on digital light processing technology. Background Art

[0002] In the aerospace field, as the requirements for aerospace engine power and efficiency continue to increase, and the need for aerospace vehicles to operate for a long time in extreme environments increases, the temperature at the engine air inlet also increases. This change makes thermal protection of high-temperature components a key issue that needs to be solved in the aerospace field, and its importance is becoming increasingly prominent.

[0003] Transpiration cooling is an active thermal protection technology with great potential. Compared with traditional thermal protection technologies, transpiration cooling has high heat protection efficiency, stable structure and can be reused as its outstanding advantages. The transpiration cooling structure can effectively absorb heat through convection and phase change mechanisms by utilizing the high specific surface area characteristics of porous media. After the coolant flows out of the porous medium, a layer of air film will be formed on the surface of the medium, producing a surface thermal resistance effect.

[0004] For example, Chinese invention patent publication numbers CN117086331A and CN117324638A use laser selective melting additive technology to prepare a metal sweating cooling structure; Chinese invention patent publication numbers CN117403118A and CN117182075A use dry pressing and hot pressing processes to prepare a porous high-temperature resistant alloy suitable for sweating cooling; Chinese invention patent publication number CN117182075A uses extrusion molding to prepare a stainless steel porous structure; the above sweating cooling structures are mainly made of metal. Although they can basically meet the current thermal protection requirements, as the flight speed and time of aircraft continue to increase, conventional metal sweating materials are difficult to withstand such high temperatures, and it is difficult to ensure long-term stable operation under the harsh conditions of high temperature and high heat flux density. In addition, metals are generally heavy, which is also an important issue for the lightweighting of aircraft.

[0005] Compared with metal sweating structures, ceramic sweating materials have the characteristics of low density, high melting point and resistance to candle burning. Academic paper: "Preparation and performance characterization of silicon carbide-based porous ceramics for sweating cooling" Silicon carbide-based porous ceramics were prepared using a foaming process; Academic paper: DOI: 10.1016 / j.ceramint.2022.04.135 C / SiC porous ceramics were prepared using a dry pressing process for sweating cooling. The foaming method and dry pressing process cannot control the distribution of the internal flow channels of the porous structure, and the mechanical properties of the prepared porous structure are low, which has a certain impact on the heat dissipation efficiency and service life of the sweating porous structure. Ceramics are difficult to process due to their high brittleness and hardness, and the sweating structure has high requirements for processing precision. Therefore, traditional processing methods are not suitable for ceramic sweating structures. Chinese Patent Publication No. CN116353834A prepares a directional porous sweating cooling structure by in-situ ceramicizing plant stem tissue. However, the in-situ ceramicizing process has high manufacturing and time costs compared to digital light processing technology and cannot be mass-produced.

[0006] Digital light processing technology provides a way to manufacture complex structures. Due to its high precision and high processing efficiency, digital light processing technology is considered to be the most suitable method for additive manufacturing of engineering ceramics. Digital light processing technology is based on ultraviolet light to cure the mixed slurry of photosensitive resin and ceramic powder, thereby stacking ceramic samples layer by layer.

[0007] Common sweating cooling porous structures are made of metal materials. Conventional metals cannot meet the growing demand for thermal barriers. Ceramic sweating materials have the characteristics of low density, high melting point and resistance to burning. Currently, SiC ceramics are used as sweating materials to manufacture sweating structure porous ceramics through dry pressing technology, but the inability to directionally control the distribution of pore size and flow channels and low mechanical properties limit its application. Summary of the invention

[0008] (I) Purpose of the invention

[0009] In order to solve the technical problems existing in the background technology, the present invention proposes a method for preparing porous ceramics with a sweating structure based on digital light processing technology. Ceramics are used as the material of the sweating structure. Ceramics have unique advantages in high temperature stability, chemical stability and mechanical properties. The use of photocuring ceramic additive process for manufacturing can ensure its molding accuracy. The appropriate sintering temperature is conducive to improving the high temperature stability and mechanical properties of porous ceramics with a sweating structure and extending its service life.

[0010] (II) Technical solution

[0011] In order to solve the above technical problems, the present invention provides a method for preparing porous ceramics with a sweating structure based on digital light processing technology, comprising the following steps:

[0012] Step S100, mixing at least two resin monomers to prepare a resin premix;

[0013] Step S200, adding a photoinitiator, a light absorber, and a plasticizer to the resin premix, and mixing them evenly to prepare a photosensitive resin;

[0014] Step S300, mixing the photosensitive resin and ceramic powder evenly to prepare a porous ceramic slurry with a sweating structure;

[0015] Step S400, slicing the designed three-dimensional model layer by layer with the same thickness to obtain a projection image of each layer, processing the projection image and setting corresponding light-curing printing conditions, adding the prepared porous ceramic slurry with a sweating structure into a digital light processing 3D printer for printing, and preparing a porous ceramic green body with a sweating structure;

[0016] Step S500, the sweating structure porous ceramic green body is subjected to degreasing and sintering processes in sequence to prepare the sweating structure porous ceramic.

[0017] Preferably, the resin monomers include cyclotrimethylolpropane formal acrylate, propoxylated neopentyl glycol diacrylate, ethoxylated trimethylolpropane triacrylate and diphthalate.

[0018] Preferably, the weight ratio of the resin premix is: 20-40 parts by weight of cyclotrimethylolpropane formal acrylate, 20-40 parts by weight of propoxylated neopentyl glycol diacrylate, 20-40 parts by weight of ethoxylated trimethylolpropane triacrylate, and 20-40 parts by weight of diphthalate.

[0019] Preferably, the photoinitiator is one or more of diacylphosphine and diphenyl phosphate;

[0020] The light absorber is one or more of dibenzoxazole ethylene and benzophenone;

[0021] The plasticizer is one or more of polyethylene glycol, polypropylene glycol and phthalate.

[0022] Preferably, the amount of photoinitiator, light absorber and plasticizer added is calculated by mass fraction, the amount of light absorber added is 0.5-1.5% of the resin premix, the amount of light absorber added is 0.01-0.03% of the resin premix, and the amount of plasticizer added is 10-30% of the resin premix.

[0023] Preferably, the ceramic powder is any one of 3 mol yttria-stabilized zirconium oxide, spherical alumina, and β-phase silicon nitride;

[0024] The particle size of the ceramic powder is 0.2-2 μm, and the solid content of the sweating structure porous ceramic slurry prepared by mixing the ceramic powder with the photosensitive resin is 48-51%.

[0025] Preferably, the mixing method of step S100 and step S200 is: using a magnetic stirrer to uniformly stir at a speed of 500 r / min for 2-4 hours;

[0026] The mixing method of step S300 is: using a centrifugal homogenizer to perform centrifugal stirring at a speed of 1000-2000 r / min until there is no powder agglomeration in the sweating structure porous ceramic slurry.

[0027] Preferably, in step S400, the thickness of the three-dimensional model sliced ​​layer by layer is 25 um;

[0028] The processing of the projection images includes: confirming whether the aperture specifications at adjacent slice projection images are the same and whether the aperture distribution positions correspond;

[0029] Two or three layers of projection slices with the same aperture specifications and aperture distribution positions are formed into a two-layer printing group or a three-layer printing group;

[0030] The single-layer printing group has differences in pore size specifications and pore size distribution positions.

[0031] Preferably, the light-curing printing parameters are: printing layer thickness 25-75 μm, scraper speed 4-6 mm / s, exposure 120-200 mJ / cm 2 , the light source wavelength is 405nm and the pixel resolution is 62.5μm.

[0032] Preferably, in step S500, the sweating structure porous ceramic green body is subjected to degreasing and sintering processes in sequence: heating from room temperature to 300-400°C at a rate of 5-60°C / h, and keeping warm for 2-4h; heating to 600-650°C at a rate of 10-30°C / h, and keeping warm for 2-4h; heating to 1450-1800°C at a rate of 120-300°C / h, and keeping warm for 2-5h; and cooling to room temperature with the furnace.

[0033] The above-mentioned technical scheme of the present invention has the following beneficial technical effects: the present invention adopts ceramic as the porous ceramic material of the sweating structure, which has better oxidation resistance and ablation resistance than the existing metal sweating structure. The present invention adopts digital light processing 3D printing technology for layering, and sets single-layer printing groups, two-layer printing groups and three-layer printing groups with different layer thicknesses by confirming whether the aperture specifications at adjacent slice projection images are the same and whether the aperture distribution positions correspond; when printing, printing groups of different thicknesses are set, and the pore walls of the printed pore structure are continuously formed, which can directionally control the pore size distribution and flow path direction in the sweating structure of the adjacent pore structure, and control the aperture specifications according to demand, so that the printing efficiency is significantly improved. Compared with the existing silicon carbide sweating structure porous ceramics manufactured by dry pressing, it is more dense and has high mechanical strength, which extends the service life of the sweating structure. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a schematic diagram of the method steps of the present invention;

[0035] Figure 2 It is a schematic diagram of the preparation process structure of the present invention. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.

[0037] like Figure 1-2 As shown, the present invention proposes a method for preparing porous ceramics with a sweating structure based on digital light processing technology, comprising the following steps:

[0038] Step S100, mixing at least two resin monomers to prepare a resin premix;

[0039] The resin monomers include cyclotrimethylolpropane formal acrylate, propoxylated neopentyl glycol diacrylate, ethoxylated trimethylolpropane triacrylate and diphthalate, which are uniformly stirred at a speed of 500 r / min for 2-4 hours using a magnetic stirrer.

[0040] It should be noted that the weight ratio of the resin premix is: 20-40 parts by weight of cyclotrimethylolpropane formal acrylate, 20-40 parts by weight of propoxylated neopentyl glycol diacrylate, 20-40 parts by weight of ethoxylated trimethylolpropane triacrylate, and 20-40 parts by weight of diphthalate.

[0041] Step S200, adding a photoinitiator, a light absorber, and a plasticizer to a resin premix, and mixing them evenly to prepare a photosensitive resin;

[0042] Wherein, the photoinitiator is one or more of diacylphosphine and diphenyl phosphate;

[0043] The light absorber is one or more of dibenzoxazole ethylene and benzophenone;

[0044] The plasticizer is one or more of polyethylene glycol, polypropylene glycol and phthalate;

[0045] Add the above materials into a magnetic stirrer and stir evenly at a speed of 500 r / min for 2-4 h.

[0046] It should be noted that the addition amounts of photoinitiator, light absorber and plasticizer are calculated by mass fraction, the addition amount of light absorber is 0.5-1.5% of the resin premix, the addition amount of light absorber is 0.01-0.03% of the resin premix, and the addition amount of plasticizer is 10-30% of the resin premix.

[0047] Step S300, mixing the photosensitive resin and the ceramic powder evenly to prepare a porous ceramic slurry with a sweating structure;

[0048] The ceramic powder is any one of 3 mol yttria-stabilized zirconium oxide, spherical alumina, and β-phase silicon nitride;

[0049] The particle size of the ceramic powder is 0.2-2 μm, and the solid content of the sweating structure porous ceramic slurry prepared by mixing the ceramic powder with the photosensitive resin is 48-51%.

[0050] Taking the mixture of 3 mol yttria-stabilized zirconia ceramic powder and photosensitive resin as an example, a centrifugal homogenizer is used to perform centrifugal stirring at a speed of 1000-2000r / min until there is no powder agglomeration in the sweating structure porous ceramic slurry, ensuring that the refractive index of the ceramic powder is close to that of the photosensitive resin, and preventing ultraviolet light from scattering in the slurry and affecting the subsequent green body molding quality.

[0051] Step S400, slicing the designed three-dimensional model layer by layer with the same thickness to obtain a projection image of each layer, processing the projection image and setting corresponding light-curing printing conditions, adding the prepared sweating structure porous ceramic slurry into a digital light processing 3D printer for printing, and preparing a sweating structure porous ceramic green body;

[0052] A three-dimensional model with the same internal and external structure specifications as the sweating structure porous ceramic is produced in the three-dimensional software according to the process parameters;

[0053] Since the optimal printing thickness of the digital light processing 3D printer is 25um, the thickness of the 3D model sliced ​​layer by layer is set to 25um, and the 3D model is sliced ​​into several layers along the vertical direction (Z axis) to obtain several projection images;

[0054] The processing of the projection images includes: confirming whether the aperture specifications at adjacent slice projection images are the same and whether the aperture distribution positions correspond;

[0055] Two or three layers of projection slices with the same aperture specifications and aperture distribution positions are formed into a two-layer printing group or a three-layer printing group;

[0056] The groups with different aperture specifications and aperture distribution positions are single-layer printing groups;

[0057] It can be understood that the layer thickness of the two-layer printing group and the three-layer printing group is 50um and 75um respectively. When the two-layer printing group and the three-layer printing group are printing, the pore structure includes straight holes and special-shaped holes with the same inclination amplitude of the pore wall. The adjacent pore structures are printed at the same time. The pore walls of the printed pore structure are continuously formed, and the pore size distribution and flow path direction in the sweating structure are directionally controlled, and the printing efficiency is significantly improved.

[0058] When printing a single-layer printing group, the printing accuracy is stable, and the pore size is controlled according to demand. The size of the prepared sweating structure porous ceramic micropores is 100μm.

[0059] It should be noted that the light-curing printing parameters are: printing layer thickness 25-75μm, scraper speed 4-6mm / s, exposure 120-200mJ / cm 2 , the light source wavelength is 405nm and the pixel resolution is 62.5μm.

[0060] Step S500, the sweating structure porous ceramic green body is subjected to degreasing and sintering processes in sequence to prepare the sweating structure porous ceramic.

[0061] Wherein, debinding includes air or nitrogen debinding, and sintering includes air or vacuum sintering;

[0062] Taking air degreasing and air sintering as an example: the degreasing and sintering procedures of the sweating structure porous ceramic green body are as follows: heating from room temperature to 300-400℃ at a rate of 5-60℃ / h, and keeping warm for 2-4h; heating to 600-650℃ at a rate of 10-30℃ / h, and keeping warm for 2-4h; heating to 1450-1800℃ at a rate of 120-300℃ / h, and keeping warm for 2-5h; cooling to room temperature with the furnace.

[0063] In this embodiment, in order to overcome the problem that the sweating cooling porous structure of metal materials cannot meet the future thermal protection needs, ceramics are used as the material of the sweating cooling porous structure. However, due to the high strength and good brittleness of ceramics and the complex structure of the sweating cooling porous material, traditional processing cannot be used for production. The present invention adopts digital light processing 3D printing technology to complete the molding of complex sweating cooling porous ceramic structures. At the same time, the micron pores in the sweating structure porous ceramics are precisely controlled so that the final pore size reaches 100μm. Ceramic powder, photosensitive resin and light absorber are used as raw materials to prepare the sweating structure porous ceramics. After subsequent post-processing such as degreasing and sintering, high-precision and dense customized manufacturing of sweating structure porous ceramics is achieved.

[0064] Embodiment 1:

[0065] Mix the resin monomer components according to weight percentage: 25% of cyclotrimethylolpropane formal acrylate, 25% of propoxylated neopentyl glycol diacrylate, 25% of ethoxylated trimethylolpropane triacrylate, and 25% of diphthalate to prepare a resin premix;

[0066] Adding 1.5% of diacylphosphine as a photoinitiator to the resin premix, adding 0.01% of dibenzoxazoleethylene as a light absorber and 10% of polyethylene glycol to the resin premix, and uniformly mixing for 3 hours using a magnetic stirrer to obtain a photosensitive resin;

[0067] The photosensitive resin and 3 mol of yttria-stabilized zirconium oxide powder are mixed with a centrifugal homogenizer at a solid content of 51% to obtain a uniform sweating structure porous ceramic slurry without powder agglomeration;

[0068] The designed three-dimensional model is sliced ​​layer by layer with the same thickness to obtain the projection image of each layer, the projection image is processed to obtain a single-layer printing group, a two-layer printing group and a three-layer printing group, and the corresponding light-curing printing conditions are set;

[0069] The single-layer printing group has a layer thickness of 25 μm, the two-layer printing group has a layer thickness of 50 μm, and the three-layer printing group has a layer thickness of 75 μm. The scraper speed is 4 mm / s and the exposure is 120 mJ / cm 2 , the wavelength of the light source is 405nm, and the pixel resolution is 62.5μm; 3D printing is performed using a 3D printing device with stereolithography technology (model: CeraStat i on 160, Jiangsu Qiandu Intelligent Manufacturing High-tech Co., Ltd.) to obtain a sweating structured porous ceramic green body.

[0070] The sweating structure porous ceramic green body is subjected to degreasing and sintering processes, the temperature is raised from room temperature to 300°C at a rate of 5°C / h, and kept warm for 3h; the temperature is raised to 600°C at a rate of 10°C / h, and the temperature is raised to 1450°C at 120°C / h, and kept warm for 4h; the temperature is cooled to room temperature along with the furnace; and a sweating structure porous zirconia ceramic is obtained.

[0071] Example 2

[0072] Mix the resin monomer components according to weight percentage: 25% of cyclotrimethylolpropane formal acrylate, 25% of propoxylated neopentyl glycol diacrylate, 25% of ethoxylated trimethylolpropane triacrylate, and 25% of diphthalate to prepare a resin premix;

[0073] Adding 1% of diacylphosphine as a photoinitiator to the resin premix, adding 0.04% of dibenzoxazoleethylene as a light absorber and 20% of polyethylene glycol to the resin premix, and uniformly mixing for 3 hours using a magnetic stirrer to obtain a photosensitive resin;

[0074] The photosensitive resin and alumina powder are mixed with a centrifugal homogenizer at a solid content of 60% to obtain a porous ceramic slurry with a uniform sweating structure and no powder agglomeration;

[0075] The designed three-dimensional model is sliced ​​layer by layer with the same thickness to obtain the projection image of each layer, the projection image is processed to obtain a single-layer printing group, a two-layer printing group and a three-layer printing group, and the corresponding light-curing printing conditions are set;

[0076] The single-layer printing group has a layer thickness of 25 μm, the two-layer printing group has a layer thickness of 50 μm, and the three-layer printing group has a layer thickness of 75 μm. The scraper speed is 4 mm / s and the exposure is 120 mJ / cm 2 , the wavelength of the light source is 405nm, and the pixel resolution is 62.5μm; 3D printing is performed using a 3D printing device with stereolithography technology (model: CeraStat i on 160, Jiangsu Qiandu Intelligent Manufacturing High-tech Co., Ltd.) to obtain a porous ceramic green body with a sweating structure;

[0077] The sweating structure porous ceramic green body is subjected to degreasing and sintering processes, and the temperature is raised from room temperature to 300°C at a rate of 10°C / h and kept at this temperature for 3 hours; the temperature is raised to 600°C at a rate of 12°C / h, and the temperature is raised to 1750°C at a rate of 120°C / h, and kept at this temperature for 4 hours; the temperature is cooled to room temperature along with the furnace; and the sweating structure porous alumina ceramic is obtained.

[0078] Example 3

[0079] Mix the resin monomer components according to weight percentage: 25% of cyclotrimethylolpropane formal acrylate, 25% of propoxylated neopentyl glycol diacrylate, 25% of ethoxylated trimethylolpropane triacrylate, and 25% of diphthalate to prepare a resin premix;

[0080] Adding 1% of diacylphosphine as a photoinitiator to the resin premix, and adding 15% of polyethylene glycol to the resin premix, and uniformly mixing for 3 hours using a magnetic stirrer to obtain a photosensitive resin;

[0081] The photosensitive resin, silicon nitride powder and sintering aid are mixed with a centrifugal homogenizer at a solid content of 50% to obtain a porous ceramic slurry with a uniform sweating structure and no powder agglomeration;

[0082] The designed three-dimensional model is sliced ​​layer by layer with the same thickness to obtain the projection image of each layer, the projection image is processed to obtain a single-layer printing group, a two-layer printing group and a three-layer printing group, and the corresponding light-curing printing conditions are set;

[0083] The single-layer printing group has a layer thickness of 25 μm, the two-layer printing group has a layer thickness of 50 μm, and the three-layer printing group has a layer thickness of 75 μm. The scraper speed is 4 mm / s and the exposure is 200 mJ / cm 2 , the wavelength of the light source is 405nm, and the pixel resolution is 62.5μm; 3D printing is performed using a 3D printing device with stereolithography technology (model: CeraStat ion 160, Jiangsu Qiandu Intelligent Manufacturing High-tech Co., Ltd.) to obtain a porous ceramic green body with a sweating structure;

[0084] The porous ceramic green body with sweating structure is subjected to nitrogen degreasing and vacuum sintering processes, and the temperature is increased from room temperature to 300°C at a rate of 60°C / h, and kept warm for 1 hour; the temperature is increased to 400°C at a rate of 30°C / h, and kept warm for 1 hour; the temperature is increased to 500°C at a rate of 30°C / h, and kept warm for 1 hour; the temperature is increased to 600°C at a rate of 30°C / h, and kept warm for 1 hour; after cooling, the degreased green body is decarburized by using a muffle furnace to increase the temperature from room temperature to 600°C at a rate of 60°C / h, and kept warm for 2 hours; the green body is cooled to room temperature; the decarburized green body is vacuum sintered in a vacuum furnace, and the temperature is increased to 1800°C at 300°C / h, and kept warm for 3 hours; the green body is cooled to room temperature by using the furnace; and the porous silicon nitride ceramic with sweating structure is obtained.

[0085] It should be emphasized that the sweating structure porous ceramics involved in this embodiment are not only suitable for the aerospace field, but can also be used for thermal protection in multiple fields such as electronic components, vehicles, and buildings. In particular, it has obvious advantages in porous ceramic sweating cooling technology for sweating structures that require customized flow channels and application scenarios with high requirements for mechanical properties.

[0086] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for preparing porous ceramics with sweating structure based on digital light processing technology, characterized in that: The following steps are involved: Step S100, mixing at least two resin monomers to prepare a resin premix; Step S200, adding a photoinitiator, a light absorber, and a plasticizer to the resin premix, and mixing them evenly to prepare a photosensitive resin; Step S300, mixing the photosensitive resin and ceramic powder evenly to prepare a porous ceramic slurry with a sweating structure; Step S400, slicing the designed three-dimensional model layer by layer with the same thickness to obtain a projection image of each layer, processing the projection image and setting corresponding light-curing printing conditions, adding the prepared porous ceramic slurry with a sweating structure into a digital light processing 3D printer for printing, and preparing a porous ceramic green body with a sweating structure; Step S500, the sweating structure porous ceramic green body is subjected to degreasing and sintering processes in sequence to prepare the sweating structure porous ceramic.

2. According to the method for preparing porous ceramics with sweating structure based on digital light processing technology in claim 1, it is characterized in that: Resin monomers include cyclotrimethylolpropane formal acrylate, propoxylated neopentyl glycol diacrylate, ethoxylated trimethylolpropane triacrylate and diphthalate esters.

3. According to the method for preparing porous ceramics with sweating structure based on digital light processing technology in claim 1, it is characterized in that: The weight ratio of the resin premix is: 20-40 parts by weight of cyclotrimethylolpropane formal acrylate, 20-40 parts by weight of propoxylated neopentyl glycol diacrylate, 20-40 parts by weight of ethoxylated trimethylolpropane triacrylate, and 20-40 parts by weight of diphthalate.

4. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: The photoinitiator is one or more of diacylphosphine and diphenyl phosphate; The light absorber is one or more of dibenzoxazole ethylene and benzophenone; The plasticizer is one or more of polyethylene glycol, polypropylene glycol and phthalate.

5. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: The added amounts of the photoinitiator, light absorber and plasticizer are calculated by mass fraction, the light absorber added amount is 0.5-1.5% of the resin premix, the light absorber added amount is 0.01-0.03% of the resin premix, and the plasticizer added amount is 10-30% of the resin premix.

6. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: The ceramic powder is any one of 3 mol yttria-stabilized zirconium oxide, spherical alumina, and β-phase silicon nitride; The particle size of the ceramic powder is 0.2-2 μm, and the solid content of the sweating structure porous ceramic slurry prepared by mixing the ceramic powder with the photosensitive resin is 48-51%.

7. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: The mixing method of step S100 and step S200 is: using a magnetic stirrer to uniformly stir at a speed of 500 r / min for 2-4 hours; The mixing method of step S300 is: using a centrifugal homogenizer to perform centrifugal stirring at a speed of 1000-2000 r / min until there is no powder agglomeration in the sweating structure porous ceramic slurry.

8. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: In step S400, the thickness of the 3D model sliced ​​layer by layer is 25 um; The processing of the projection images includes: confirming whether the aperture specifications at adjacent slice projection images are the same and whether the aperture distribution positions correspond; Two or three layers of projection slices with the same aperture specifications and aperture distribution positions are formed into a two-layer printing group or a three-layer printing group; The single-layer printing group has differences in pore size specifications and pore size distribution positions.

9. The method for preparing porous ceramics with a sweating structure based on digital light processing technology according to claim 8, characterized in that: The light-curing printing parameters are: printing layer thickness 25-75μm, scraper speed 4-6mm / s, exposure 120-200mJ / cm 2 , the light source wavelength is 405nm and the pixel resolution is 62.5μm.

10. The method for preparing porous ceramics with sweating structure based on digital light processing technology according to claim 1, characterized in that: In step S500, the sweating structure porous ceramic green body is degreased and sintered in sequence: heating from room temperature to 300-400°C at a rate of 5-60°C / h, and keeping warm for 2-4h; heating to 600-650°C at a rate of 10-30°C / h, and keeping warm for 2-4h; heating to 1450-1800°C at a rate of 120-300°C / h, and keeping warm for 2-5h; and cooling to room temperature with the furnace.

Citation Information

Patent Citations

  • Additive manufacturing composite layered slicing method

    CN110253890A

  • Preparation method of cross-scale porous material

    CN116693322A

  • Rapid preparation method of water-soluble mold core based on digital light processing technology

    CN117620097A

  • Preparation method of bionic gradient stent and bionic gradient stent

    CN118000973A

  • High porosity material and method of making thereof

    US20170284206A1

Cited By

  • Sweat removing type heat dissipation method and system for server or intelligent robot

    CN120973203A