Carbon / carbon composite material and preparation method and application thereof
Through the combination of polyolefin and cyclized organic fibers, chemical cross-linking and pyrolysis are used to solve the problems of long curing cycle and complex molding process in the preparation of carbon/carbon composite materials, and achieve the improvement of material performance and cost reduction. reduce.
Patent Information
- Application Number
- CN202410984702.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-11
AI Technical Summary
In the existing preparation process of carbon/carbon composite materials, the resin matrix has a long curing cycle, complex molding process, and high porosity, resulting in insufficient material performance and low preparation cost and time efficiency.
Polyolefin is used as the matrix resin and cyclized organic fiber as the reinforcement. Through chemical cross-linking treatment, pyrolysis treatment, carburization treatment and siliconization treatment, combined with densification treatment, carbon/carbon composite materials are prepared to realize the matrix resin and fiber The synchronous shrinkage of the reinforcement suppresses crack defects and improves mechanical properties and density.
It effectively shortens the preparation cycle, reduces costs, improves the mechanical properties, wave absorption performance and oxidation resistance of carbon/carbon composite materials, and simplifies the molding process.
Smart Images

Figure CN118754696A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of composite materials and relates to a carbon / carbon composite material and a preparation method and application thereof. Background Art
[0002] Carbon fiber reinforced carbon-based (abbreviated as carbon / carbon or C / C) composites have excellent properties such as high strength, low density, high fracture toughness, excellent chemical resistance, good thermal shock resistance and ablation resistance at high temperatures, and have been used as thermal protection systems in certain extreme conditions. Silicon carbide (SiC) is a non-oxide ceramic that is compatible with carbon. The addition of SiC can improve the oxidation resistance of C / C composites. Carbon fiber reinforced carbon and silicon carbide composites (C / C–SiC) have high thermomechanical loads and show excellent properties of high specific mechanical strength, thermal stability, damage tolerance, wear resistance and thermal shock resistance. They are excellent materials for thermal protection systems. In addition, the introduction of SiC components can improve the interfacial polarization loss capacity of the composite material, significantly improve the wave absorption performance of the composite material, and expand the application scenarios of C / C-SiC composites.
[0003] C / C composite material is prepared by carbonization and densification process of carbon fiber reinforced resin-based composite material, and C / C-Si C composite material is introduced SiC component on the basis of C / C composite material. Therefore, the precursors of C / C composite material and C / C-Si C composite material are all carbon fiber reinforced resin-based composite material. Phenolic resin has become one of the most commonly used polymer resin matrices at present because of its advantages such as easy processing, low price and high carbon content, but the curing cycle of phenolic resin is long, the porosity is high and the process is complicated. In view of the above problems, patent CN 107879758 A designs a novel sandwich structure composite material with high-density C / C in the middle and symmetrically distributed C / C-SiC and C-SiC on both sides. This process effectively reduces the preparation cost of C / C-SiC material and shortens the preparation cycle. In order to solve the problem of high porosity of C / C-SiC composite materials, patent CN 114645449 A discloses a method for modifying C / C-SiC composite materials with polyimide resin carbon. By introducing a polyimide resin carbon layer, the pore structure of the C / C composite matrix is adjusted and the density of the composite material is enhanced.
[0004] However, although the existing patented technology has effectively reduced the preparation cost of C / C and C / C-SiC composite materials, optimized the preparation process and shortened the preparation cycle, it still has not effectively solved the problems of long resin matrix curing cycle and complex molding process.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a carbon / carbon composite material and a preparation method and application thereof, so as to solve the above-mentioned technical problems existing in the prior art.
[0007] In order to achieve the above purpose, the following technical solutions are adopted:
[0008] The first object of the present invention is to provide a method for preparing a carbon / carbon composite material, comprising the following steps:
[0009] (a) using polyolefin as a matrix resin and cyclized organic fiber as a reinforcement to prepare a carbon / carbon composite material precursor; wherein the polyolefin is a polyolefin that can be carbonized after chemical crosslinking and pyrolysis treatment;
[0010] (b) chemically cross-linking the carbon / carbon composite material precursor to obtain an infusible intermediate;
[0011] (c) subjecting the infusible intermediate to a first pyrolysis treatment to obtain a carbon / carbon material;
[0012] (d) subjecting the infusible intermediate of step (b) or the carbon / carbon material of step (c) to carburizing and / or siliconizing to obtain an infiltration product;
[0013] (e) subjecting the infiltration product to a second pyrolysis treatment and an optional densification treatment to obtain a carbon / carbon composite material;
[0014] The preparation temperature of the cyclized organic fiber in step (a) is lower than the pyrolysis temperature of the first pyrolysis treatment in step (c) and the pyrolysis temperature of the second pyrolysis treatment in step (e).
[0015] Further, on the basis of the above technical solution of the present invention, in step (a), the polyolefin includes polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyvinyl norbornene homopolymer and its grafted modified products or carbon nanofiller modified products, or one or more of binary, ternary, or multi-polymers containing the above homopolymer structural units and its grafted modified products or carbon nanofiller modified products; preferably, the grafted modified product of the polyolefin homopolymer or copolymer is a modified product obtained by grafting the polyolefin homopolymer or copolymer with a polar monomer, and the polar monomer includes at least one of maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene;
[0016] Preferably, the carbon nanofiller-modified product of the polyolefin homopolymer or copolymer is a modified product of the polyolefin homopolymer or copolymer modified with a carbon nanofiller, and the carbon nanofiller includes at least one of carbon nanotubes, alkyl-modified carbon nanotubes, siloxane-modified carbon nanotubes, graphene nanosheets, alkyl-modified graphene nanosheets, graphene oxide or graphite.
[0017] Further, on the basis of the above technical solution of the present invention, the cyclized organic fiber includes one or more of polyacrylonitrile-based carbon fiber, pre-oxidized polyacrylonitrile fiber, asphalt-based carbon fiber, pre-oxidized asphalt fiber, viscose-based carbon fiber, pre-oxidized viscose fiber, lignin-based carbon fiber, pre-oxidized lignin fiber, polyimide-based carbon fiber, polyimide fiber, polyethylene-based carbon fiber, sulfonated polyethylene fiber, polypropylene-based carbon fiber or sulfonated polypropylene fiber;
[0018] Preferably, the carbonization temperature of the polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, viscose-based carbon fiber, lignin-based carbon fiber, polyimide-based carbon fiber, polyethylene-based carbon fiber and polypropylene-based carbon fiber is 400-1200°C, preferably 400-900°C.
[0019] Further, on the basis of the above technical solution of the present invention, the cyclized organic fiber exists in the form of short-cut fibers and / or continuous fibers, wherein the length of the short-cut fibers is 0.03 mm-30 mm;
[0020] And / or, the mass ratio of the cyclized organic fiber to the polyolefin is (0.1-90):100.
[0021] Further, on the basis of the above technical solution of the present invention, in step (b), the chemical cross-linking treatment includes one or more of sulfonation treatment, thermal oxidation treatment, ammonia oxidation treatment, bromination treatment, plasma treatment, irradiation treatment or sulfurization treatment;
[0022] And / or, in step (c), the pyrolysis temperature of the first pyrolysis treatment is 700-3000° C., the pyrolysis time is 10 min-180 min, and the pyrolysis is carried out in a protective atmosphere.
[0023] Further, on the basis of the above technical solution of the present invention, in step (d), the infusible intermediate or the carbon / carbon material is immersed in a carbon precursor solution for carburizing treatment and / or immersed in a silicon-containing precursor solution for siliconizing treatment;
[0024] Preferably, the carbon precursor in the carbon precursor solution includes one or more of asphalt, lignin, polyacrylonitrile or phenolic resin;
[0025] Preferably, the solvent in the carbon precursor solution includes one or more of carbon tetrachloride, toluene, dimethyl sulfoxide or acetone;
[0026] Preferably, the carbon precursor accounts for 0-60% of the total mass of the infiltration product obtained after carburizing treatment;
[0027] Preferably, the specific steps of the carburizing treatment include: immersing the infusible intermediate or carbon / carbon material in a carbon precursor solution for 5-180 minutes, and then performing a thermal stabilization treatment at 50-300° C. for 1-20 hours.
[0028] Further, on the basis of the above technical solution of the present invention, in step (d), the silicon-containing precursor in the silicon-containing precursor solution includes one or more of n-tetramethylsilane, polycarbosilane or element-doped polycarbosilane, wherein the element doped in the element-doped polycarbosilane includes at least one of boron, titanium, aluminum, iron, cobalt, nickel or zirconium;
[0029] and / or, the silicon-containing precursor accounts for 0-50% of the total mass of the infiltration product obtained after siliconizing treatment;
[0030] And / or, the specific steps of the siliconizing treatment include: immersing the infusible intermediate or the carbon / carbon material or the infiltration product obtained after the carburizing treatment in a silicon-containing precursor solution for 5-180 minutes, and then drying at 50-200° C. for 1-20 hours.
[0031] Further, on the basis of the above technical solution of the present invention, in step (e), the pyrolysis temperature of the second pyrolysis treatment is 500-2650° C., the pyrolysis time is 0.1-5 h, and the pyrolysis is carried out in a protective atmosphere;
[0032] and / or, in step (e), the densification treatment includes the step of impregnating the pyrolysis product obtained after the second pyrolysis treatment in the carbon precursor solution and / or the silicon-containing precursor solution in step (d), and then pyrolyzing it again;
[0033] And / or, the densification treatment is performed 0-10 times.
[0034] The second object of the present invention is to provide a carbon / carbon composite material, which is prepared by the above-mentioned method for preparing the carbon / carbon composite material.
[0035] The third object of the present invention is to provide a method for preparing the above-mentioned carbon / carbon composite material or the application of the above-mentioned carbon / carbon composite material in the fields of aerospace, automobile manufacturing or energy.
[0036] Compared with the prior art, the technical solution of the present invention has at least the following technical effects:
[0037] (1) The present invention provides a method for preparing a carbon / carbon composite material, wherein a polyolefin is used as a matrix resin and a cyclized organic fiber is used as a reinforcement to prepare a carbon / carbon composite material precursor, and the carbon / carbon composite material precursor is subjected to a chemical crosslinking treatment, an optional first pyrolysis treatment, a carburizing treatment and / or a siliconizing treatment, and a second pyrolysis treatment and an optional densification treatment to obtain a carbon / carbon composite material; wherein the matrix resin (polyolefin) and the fiber reinforcement (cyclized organic fiber) can achieve synchronous shrinkage during the pyrolysis process, which can effectively inhibit the generation of crack defects in the carbon / carbon composite material, and is beneficial to the improvement of the mechanical properties of the carbon / carbon composite material; at the same time, the use of a polyolefin thermoplastic resin as a matrix resin effectively solves the problems of a long curing cycle and a complex molding process of a traditional matrix resin (such as a phenolic resin).
[0038] (2) The present invention provides a carbon / carbon composite material, which is prepared by the preparation method of the carbon / carbon composite material of the present invention. In view of the advantages of the above-mentioned preparation method, the prepared carbon / carbon composite material has good mechanical properties, wave absorption properties and antioxidant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0040] Figure 1 These are morphology pictures of the carbon / carbon composite materials prepared in Example 1, Comparative Example 1 and Comparative Example 3 of the present invention, wherein (a) corresponds to Comparative Example 3, (b) corresponds to Comparative Example 1, and (c) corresponds to Example 1. DETAILED DESCRIPTION
[0041] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.
[0042] The endpoints and any values of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.
[0043] According to a first aspect of the present invention, there is provided a method for preparing a carbon / carbon composite material, comprising the following steps:
[0044] (a) using polyolefin as a matrix resin and cyclized organic fiber as a reinforcement to prepare a carbon / carbon composite material precursor; wherein the polyolefin is a polyolefin that can be carbonized after chemical crosslinking and pyrolysis treatment;
[0045] (b) chemically cross-linking the carbon / carbon composite material precursor to obtain an infusible intermediate;
[0046] (c) subjecting the infusible intermediate to a first pyrolysis treatment to obtain a C / C material;
[0047] (d) subjecting the infusible intermediate of step (b) or the C / C material of step (c) to carburizing and / or siliconizing to obtain an infiltration product;
[0048] (e) subjecting the impregnated product to a second pyrolysis treatment under an inert atmosphere, and optionally to a densification treatment, to obtain a carbon / carbon composite material;
[0049] The preparation temperature of the cyclized organic fiber in step (a) is lower than the pyrolysis temperature of the first pyrolysis treatment in step (c) and the pyrolysis temperature of the second pyrolysis treatment in step (e).
[0050] Specifically, in step (a), the type of polyolefin is selected from polyolefins that can be carbonized after chemical crosslinking and pyrolysis. If chemical crosslinking is not possible, it will decompose into small molecular gases after high-temperature pyrolysis, and carbon / carbon composite materials cannot be obtained. It should be noted that the chemical crosslinking treatment mentioned above can be understood as the chemical crosslinking treatment in step (b) of the present invention, and the pyrolysis treatment mentioned above can be understood as the first pyrolysis treatment in step (c) of the present invention and the second pyrolysis treatment in step (e). For example, the type of polyolefin can be polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, polyisoprene, poly-1-hexene, etc. that are common in the art. Using polyolefin as a resin matrix has low raw material cost, not only has a high carbon content, but also can obtain a product with a high carbon yield after appropriate chemical crosslinking treatment (crosslinking infusible method) in step (b).
[0051] Cyclized organic fiber refers to an organic fiber with a cross-linked network structure, which is derived from a multi-ring structure formed by cross-linking between molecules inside a linear polymer, or a multi-ring structure formed by cross-linking between molecules of a condensed ring polymer. The cyclized organic fiber can be converted into a carbon fiber after further high-temperature carbonization. The preparation temperature for converting it into a carbon fiber is usually 400-1200°C, which is lower than the carbonization temperature of ordinary carbon fiber (1300-1500°C). Using cyclized organic fiber as a reinforcement can not only withstand high temperatures and strong acids, but also achieve synchronous shrinkage of the matrix resin and the fiber reinforcement during the preparation of carbon / carbon composite materials, inhibit the expansion of crack defects during the preparation of carbon / carbon composite materials, and help improve the mechanical properties of carbon / carbon composite materials.
[0052] The carbon / carbon composite material precursor is a composite material formed by cyclized organic fibers and polyolefins. The preparation method thereof is not specifically limited and it can be rapidly formed by hot pressing, extrusion, injection molding or 3D printing, etc., and has the advantage of a simple preparation process.
[0053] In step (b), the carbon / carbon composite material precursor is chemically cross-linked so that the resin matrix is transformed from a linear structure to a highly cross-linked cyclic structure, and the cyclic organic fibers are not further carbonized during this process.
[0054] The infusible intermediate in step (b) can be subjected to a first pyrolysis treatment (i.e., step (c)) to obtain a carbon / carbon material, and then subjected to a carburizing treatment and / or a siliconizing treatment (i.e., step (d)). Alternatively, the infusible intermediate can be subjected to a first pyrolysis treatment (i.e., step (c)) to obtain a carbon / carbon material, and then subjected to a carburizing treatment and / or a siliconizing treatment (i.e., step (d)) without being subjected to a first pyrolysis treatment.
[0055] In step (d), the purpose of carburizing the infusible intermediate or carbon / carbon material is to improve the compactness of the material. The purpose of carburizing and siliconizing the infusible intermediate or carbon / carbon material is, on the one hand, to improve the compactness of the material, and on the other hand, to introduce a silicon-containing compound (silicon source) to react with carbon to form a SiC phase in a subsequent step.
[0056] It should be noted that the "carburizing and / or siliconizing treatment" in step (d) means that the infusible intermediate or carbon / carbon material can be subjected to only carburizing treatment, only siliconizing treatment, or both carburizing treatment and siliconizing treatment.
[0057] In step (e), the infiltration product (carburized product, siliconized product or carburized siliconized product) is placed in an inert atmosphere for pyrolysis (second pyrolysis treatment) to perform pyrolysis carbonization to form a carbon / carbon composite material. Wherein, the siliconized product or carburized siliconized product is placed in an inert atmosphere for pyrolysis, and the silicon-containing compound (silicon source) in the siliconized product or carburized siliconized product interacts with carbon to form a SiC phase during the high-temperature pyrolysis process, and a carbon / carbon composite material containing a SiC phase can be obtained.
[0058] Moreover, it should be noted that since the preparation temperature of the cyclized organic fibers in the impregnation product is lower than the pyrolysis temperature in step (c) and step (e), during the pyrolysis process of step (c) and step (e), the cyclized organic fibers in the infusible intermediate or the impregnation product and the resin matrix will pyrolyze and shrink synchronously, thereby inhibiting the expansion of crack defects.
[0059] Densification treatment is mainly used to reduce defects of carbon / carbon composite materials and improve the density, mechanical properties and anti-oxidation properties of the composite materials. "Optional densification treatment" means that densification treatment may or may not be performed, and is set according to actual needs.
[0060] The present invention adopts cyclized organic fibers as reinforcements, and can achieve controllable adjustment of the content of non-carbon impurity elements in the resin matrix and the fiber reinforcement by regulating the pyrolysis temperature during the preparation of the carbon / carbon composite material, thereby giving the carbon / carbon composite material additional functional properties such as wave absorption and electrochemistry.
[0061] The present invention uses a cross-linked infusible intermediate or a pyrolyzed carbon / carbon material as a precursor for carburizing and / or siliconizing, which can provide the gaps necessary for carburizing and / or siliconizing, effectively increase the carbon / carbon or silicon-carbon contact area, increase the carbon thermal reaction sites, and promote the conversion process of carbon / carbon or silicon carbide during pyrolysis.
[0062] The simplified molding process and low raw material cost of this method will provide a feasible solution for large-scale production.
[0063] As an optional embodiment of the present invention, in step (a), the polyolefin includes polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyvinyl norbornene homopolymer or the above homopolymers (for example, polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyvinyl norbornene homopolymer) . One or more of the grafted modified products of polyethylene norbornene, polyethylene norbornene homopolymer) or carbon nanofiller modified products, or binary, ternary, or multi-polymers containing the above homopolymer structural units (for example, ethylene-propylene copolymers, ethylene-butene copolymers, ethylene-pentene copolymers, ethylene-butene-pentene copolymers, ethylene-propylene-butene copolymers, ethylene-propylene-ene-pentene copolymers, etc.) or the above copolymers (binary, ternary, or multi-polymers containing the above homopolymer structural units) or one or more of the grafted modified products of the carbon nanofiller modified products.
[0064] It should be noted that the graft-modified product of the above-mentioned homopolymer or the graft-modified product of the above-mentioned copolymer mainly refers to the modified product obtained by grafting and modifying the polyolefin homopolymer or copolymer with a polar monomer (such as maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene, etc.); the carbon nanofiller-modified product of the above-mentioned homopolymer or the carbon nanofiller-modified product of the above-mentioned copolymer mainly refers to the modified product obtained by blending and modifying the polyolefin homopolymer or copolymer with a carbon nanofiller (such as carbon nanotubes, alkyl-modified carbon nanotubes, siloxane-modified carbon nanotubes, graphene nanosheets, alkyl-modified graphene nanosheets, graphene oxide, graphite, etc.).
[0065] As an optional embodiment of the present invention, in step (a), the cyclized organic fiber includes one or more of polyacrylonitrile-based carbon fiber, pre-oxidized polyacrylonitrile fiber, asphalt-based carbon fiber, pre-oxidized asphalt fiber, viscose-based carbon fiber, pre-oxidized viscose fiber, lignin-based carbon fiber, pre-oxidized lignin fiber, polyimide-based carbon fiber, polyimide fiber, polyethylene-based carbon fiber, sulfonated polyethylene fiber, polypropylene-based carbon fiber or sulfonated polypropylene fiber.
[0066] As a preferred embodiment of the present invention, the carbonization temperature (preparation temperature) in the preparation process of polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, viscose-based carbon fiber, lignin-based carbon fiber, polyimide-based carbon fiber, polyethylene-based carbon fiber and polypropylene-based carbon fiber is lower than the pyrolysis temperature in step (d), preferably 400-1200°C (for example, 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C or 1200°C, etc. and the numerical range between any two points), further preferably 400-900°C.
[0067] As a preferred embodiment of the present invention, preoxidized polyacrylonitrile fiber, preoxidized asphalt fiber, preoxidized viscose fiber, preoxidized lignin fiber, polyimide fiber, sulfonated polyethylene fiber and sulfonated polypropylene fiber are all uncarbonized fibers, which can gradually remove non-carbon elements during the carbonization process to form carbon fibers.
[0068] As an optional embodiment of the present invention, in step (a), the cyclized organic fibers are in the form of chopped fibers and / or continuous fibers, wherein the length of the chopped fibers is 0.03 mm to 30 mm.
[0069] As an optional embodiment of the present invention, in step (a), the mass ratio of the cyclized organic fiber to the polyolefin is (0.1-90): 100. Typical but non-limiting mass ratios of the cyclized organic fiber to the polyolefin are 0.1:100, 0.5:100, 1:100, 5:100, 10:100, 20:100, 30:100, 40:100, 50:100, 60:100, 70:100, 80:100 or 90:100, etc.
[0070] As an optional embodiment of the present invention, in step (a), the carbon / carbon composite material precursor includes fiber-reinforced polyolefin fibers, films, rods, profiles, special-shaped materials, components and other fiber-reinforced polyolefin materials with one-dimensional, two-dimensional and three-dimensional dimensional structural characteristics prepared by melt spinning, hot pressing, extrusion, injection molding, blow molding, compression or 3D printing, and can also be subjected to additive and subtractive processing, mechanical processing and melt connection.
[0071] As an optional embodiment of the present invention, in step (b), the chemical cross-linking treatment includes one or more of sulfonation treatment, thermal oxidation treatment, ammonia oxidation treatment, bromination treatment, plasma treatment, irradiation treatment or vulcanization treatment.
[0072] Among them, the sulfonation treatment mainly uses sulfur trioxide, fuming sulfuric acid, chlorosulfonic acid, sulfuric acid or their complexes to carry out sulfonation cross-linking treatment on polyolefins to make them cyclodehydrogenate to form a high-temperature insoluble multi-cyclic structure.
[0073] Thermal oxidation treatment mainly uses hot air to oxidatively crosslink polyolefins to cause them to undergo oxidative dehydrogenation to form a multi-ring structure that is insoluble at high temperatures.
[0074] Ammoxidation treatment mainly involves thermal oxidation crosslinking of polyolefins in the presence of ammonia to dehydrogenate them to form a multi-ring structure that is insoluble at high temperatures.
[0075] Bromination treatment mainly uses liquid bromine to carry out liquid phase bromination dehydrogenation treatment on polyolefins under heating conditions to form a multi-ring structure that is insoluble at high temperature.
[0076] Plasma treatment mainly uses plasma to treat polyolefins to generate highly reactive free radicals, which can more easily induce sulfonation cross-linking reactions.
[0077] Irradiation treatment mainly uses electron beam radiation to irradiate polyolefins to generate highly reactive free radicals, which can more easily induce sulfonation cross-linking reactions.
[0078] The vulcanization treatment mainly uses sublimated sulfur to perform a vulcanization and dehydrogenation treatment on polyolefins to form a high-temperature insoluble multi-ring structure.
[0079] The chemical cross-linking treatment is mainly used to convert the polyolefin into a cyclic structure and to improve the carbon yield of the base resin.
[0080] As an optional embodiment of the present invention, in step (c), the pyrolysis temperature of the first pyrolysis treatment is 700-3000°C, the pyrolysis time is 10min-180min, and the pyrolysis is carried out in a protective atmosphere. Typical but non-limiting pyrolysis temperatures are 700°C, 800°C, 1000°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1800°C, 2000°C, 2200°C, 2300°C, 2400°C, 2500°C, 2600°C, 2800°C, 2900°C or 3000°C, and the numerical range between any two points. Typical but non-limiting pyrolysis times are 10min, 20min, 30min, 50min, 1h, 1.5h, 2h, 2.5h or 3h, etc. The protective atmosphere includes at least one of nitrogen, argon or helium.
[0081] As an optional embodiment of the present invention, in step (d), the infusible intermediate or the carbon / carbon material is immersed in a carbon precursor solution for carburizing treatment and / or immersed in a silicon-containing precursor solution for siliconizing treatment.
[0082] As an optional embodiment of the present invention, in step (d), the carbon precursor in the carbon precursor solution includes one or more of asphalt, lignin, polyacrylonitrile or phenolic resin.
[0083] As an optional embodiment of the present invention, in step (d), the solvent in the carbon precursor solution includes one or more of carbon tetrachloride, toluene, dimethyl sulfoxide or acetone.
[0084] As an optional embodiment of the present invention, in step (d), the carbon precursor accounts for 0-60% of the total mass of the infiltration product (carburized product). Typical but non-limiting mass fractions of the carbon precursor in the infiltration product are 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55% or 60%, etc. and the numerical range between any two points.
[0085] By further limiting the specific composition of the carbon precursor solution and the mass fraction of the carbon precursor in the infiltration product, the carbon yield and elemental composition of the carbon / carbon composite material can be better regulated, giving the carbon / carbon composite material excellent functional properties.
[0086] As an optional embodiment of the present invention, the specific steps of carburizing treatment include: placing the infusible intermediate or carbon / carbon material or the siliconized product after siliconization treatment in a carbon precursor solution for 5-180 minutes, and then heat stabilizing it at 50-300° C. for 1-20 hours. The heat stabilization treatment is performed to dry the impregnated product (the infusible intermediate or carbon / carbon material after impregnation or the siliconized product after siliconization treatment) on the one hand, and on the other hand, the carbon precursor attached to the product undergoes an oxidative cross-linking reaction in an air atmosphere, thereby achieving carbonization in the subsequent pyrolysis process.
[0087] Typical but non-limiting immersion times are 5 min, 10 min, 20 min, 40 min, 50 min, 60 min, 80 min, 100 min, 120 min, 140 min, 150 min, 160 min or 180 min, etc., typical but non-limiting heat stabilization temperatures are 50°C, 60°C, 80°C, 100°C, 120°C, 150°C, 180°C, 200°C, 230°C, 250°C, 270°C or 300°C, etc., typical but non-limiting heat stabilization times are 1 h, 2 h, 5 h, 6 h, 8 h, 12 h, 15 h, 16 h, 18 h or 20 h, etc.
[0088] By further limiting the specific steps of the carburizing treatment, the density of the carbon / carbon composite material is improved.
[0089] As an optional embodiment of the present invention, in step (d), the silicon-containing precursor in the silicon-containing precursor solution includes one or more of n-tetramethylsilane, polycarbosilane or element-doped polycarbosilane. Wherein, the element doped in the element-doped polycarbosilane includes at least one of boron, titanium, aluminum, iron, cobalt, nickel or zirconium, and the mass fraction of the doped element in the polycarbosilane is 0.5-20% (e.g., 0.5%, 1%, 2%, 4%, 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18% or 20%, etc.).
[0090] By using element-doped polycarbosilane as a silicon-containing precursor, metal doping of carbon / carbon composite materials (carbon / carbon-silicon carbide composite materials) containing silicon carbide phases can be achieved, thereby improving the wave absorbing performance of the material.
[0091] As an optional embodiment of the present invention, in step (d), the silicon-containing precursor accounts for 0-50% of the total mass of the infiltration product (siliconized product). Typical but non-limiting mass fractions of the silicon-containing precursor in the infiltration product are 0%, 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc. and the range of values between any two points.
[0092] By further limiting the specific composition of the silicon-containing precursor solution and the mass fraction of the silicon-containing precursor in the infiltration product, the SiC phase content in the carbon / carbon composite material can be better regulated, which is beneficial to balancing the mechanical properties and antioxidant properties of the carbon / carbon composite material.
[0093] As an optional embodiment of the present invention, in step (d), the specific step of siliconizing treatment includes: placing the infusible intermediate or carbon / carbon material or the carburized product after carburizing treatment in a silicon-containing precursor solution for 5-180 minutes, and then drying it at 50-200° C. for 1-20 hours. Typical but non-limiting immersion times are 5 minutes, 10 minutes, 20 minutes, 40 minutes, 50 minutes, 60 minutes, 80 minutes, 100 minutes, 120 minutes, 140 minutes, 150 minutes, 160 minutes or 180 minutes, etc., typical but non-limiting drying temperatures are 50° C., 60° C., 80° C., 100° C., 120° C., 150° C., 180° C. or 200° C., etc., and typical but non-limiting drying times are 1 hour, 2 hours, 5 hours, 6 hours, 8 hours, 12 hours, 15 hours, 16 hours, 18 hours or 20 hours, etc.
[0094] By further limiting the specific steps of siliconizing treatment, the density of the carbon / carbon composite material is improved.
[0095] As an optional embodiment of the present invention, in step (e), the pyrolysis temperature of the second pyrolysis treatment is 500-2650°C, the pyrolysis time is 0.1-5h, and the pyrolysis is carried out in a protective atmosphere. Typical but non-limiting pyrolysis temperatures are 500°C, 600°C, 800°C, 1000°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1800°C, 2000°C, 2200°C, 2300°C, 2400°C, 2500°C, 2600°C or 2650°C, and the numerical range between any two points. Typical but non-limiting pyrolysis times are 0.1h, 0.5h, 1h, 2h, 3h, 4h or 5h, etc. Typical but non-limiting pyrolysis atmospheres include nitrogen, argon, helium or neon, etc.
[0096] As an optional embodiment of the present invention, in step (e), the densification treatment includes the step of impregnating the pyrolysis product in the carbon precursor solution and / or the silicon-containing precursor solution of step (d), and then pyrolyzing. It should be noted that when it is necessary to impregnate both the carbon precursor solution and the silicon-containing precursor solution, there is no special requirement for the impregnation order, and it can be first impregnated in the carbon precursor solution and then in the silicon-containing precursor solution, or first impregnated in the silicon-containing precursor solution and then in the carbon precursor solution.
[0097] As an optional embodiment of the present invention, the number of densification treatments is 0-10 times. It should be noted that when the number of densification treatments is 0 times, it indicates that after the step (e) pyrolyzes the infiltration product (carburized product, siliconized product or carburized siliconized product) under an inert atmosphere, there is no need to perform densification treatment, and a carbon / carbon composite material is directly obtained. When the number of densification treatments is 1 time, that is, after the step (e) pyrolyzes the infiltration product under an inert atmosphere, the obtained pyrolysis product is impregnated in the carbon precursor solution and / or silicon-containing precursor solution of step (d), and then pyrolyzed again, carbon / carbon and or carbon / carbon-silicon carbide composite materials are obtained. When the number of densification treatments is other times, by analogy, it will not be repeated here.
[0098] According to a second aspect of the present invention, there is also provided a carbon / carbon composite material, which is prepared by the above-mentioned method for preparing the carbon / carbon composite material.
[0099] The preparation method of the carbon / carbon composite material of the present invention adopts polyolefin as a matrix resin and cyclized organic fiber as a reinforcement to prepare a carbon / carbon composite material precursor, and obtains the carbon / carbon composite material by subjecting the carbon / carbon composite material precursor to a chemical crosslinking treatment, an optional first pyrolysis treatment, a carburizing treatment and / or a siliconizing treatment, a second pyrolysis treatment and an optional densification treatment; wherein the matrix resin and the fiber reinforcement can achieve synchronous shrinkage during the pyrolysis process, which can effectively inhibit the generation of crack defects in the carbon / carbon composite material, and is beneficial to the improvement of the mechanical properties of the carbon / carbon composite material; at the same time, the use of polyolefin thermoplastic resin as the matrix resin effectively solves the problems of long curing cycle and complex molding process of traditional matrix resins (such as phenolic resin).
[0100] According to a third aspect of the present invention, there is also provided a method for preparing the above carbon / carbon composite material or the application of the above carbon / carbon composite material in the fields of aerospace, automobile manufacturing or energy.
[0101] The preparation method provided by the present invention will help promote the development of carbon / carbon composite materials and be widely used in aerospace, automobile manufacturing, energy fields, etc. At the same time, the simplified molding process and low raw material cost of the method will provide a feasible solution for large-scale production, further promoting the market popularization and application expansion of the composite material.
[0102] The present invention is further described in detail below in conjunction with specific examples and comparative examples. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Unless otherwise specified, the raw materials used in the present invention can all be obtained from commercially available products. Specific raw material information is shown in Table 1.
[0103] Table 1
[0104]
[0105]
[0106] At the same time, the cyclized organic fibers (polyimide-based carbon fibers, pre-oxidized polyacrylonitrile fibers, polyacrylonitrile-based carbon fibers, polyacrylonitrile-based carbon nanofibers, sulfonated polypropylene fibers, polypropylene-based carbon fibers, pre-oxidized lignin fibers, lignin-based carbon fibers, pre-oxidized asphalt fibers, asphalt-based carbon fibers, sulfonated polyethylene fibers, polyethylene-based carbon fibers, pre-oxidized viscose fibers, viscose-based carbon fibers) and element-doped polycarbosilanes (cobalt-doped polycarbosilanes, nickel-doped polycarbosilanes, and iron-doped polycarbosilanes) involved in the embodiments of the present invention and the comparative examples are all homemade in the laboratory, and the specific preparation methods are as follows. Preparation of polyimide-based carbon fibers:
[0107] The commercially available polyimide fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at a preset carbonization temperature of 1200°C for 10 min to prepare a polyimide-based carbon fiber.
[0108] Preparation of pre-oxidized polyacrylonitrile fiber and polyacrylonitrile-based carbon fiber:
[0109] Polyacrylonitrile fiber was prepared by wet spinning: the polyacrylonitrile spinning stock solution was precisely filtered and measured, extruded from a 3K spinneret, and coagulated in a dimethyl sulfoxide aqueous solution. The coagulated polyacrylonitrile primary fiber was stretched and washed with hot water, and then squeezed with a rubber roller to remove moisture from the surface of the fiber bundle. The fiber was quickly placed in a vertical oven and kept at 80°C, 100°C, and 120°C for 80s, 100s, and 180s, respectively. The heating rate was 5°C / min to achieve drying and densification of the fiber, thereby preparing dry and densified polyacrylonitrile fiber.
[0110] The prepared polyacrylonitrile fiber was placed in an oven for pre-oxidation, with the residence times at 220°C, 240°C, 260°C and 280°C being 30 min, 30 min, 30 min and 120 min respectively, and the heating rate being 5°C / min, to prepare pre-oxidized polyacrylonitrile fiber.
[0111] The prepared pre-oxidized polyacrylonitrile fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and kept at a preset carbonization temperature of 700°C for 10 min to prepare polyacrylonitrile-based carbon fiber.
[0112] Preparation of polyacrylonitrile-based carbon nanofibers:
[0113] N,N-dimethylformamide was used as a solvent to prepare a 15wt% spinning solution, which was injected into a syringe, and then a propeller was installed on the propulsion device, and aluminum foil was used to collect the fibers. The voltage was set to 15KV, the propeller speed was 1ml / h, the receiver drum speed was 1300r / min, and the fibers were collected for 2h to prepare a polyacrylonitrile nanofiber membrane.
[0114] The prepared polyacrylonitrile nanofiber membrane was placed in an oven for pre-oxidation. The residence times at 220°C, 240°C, 260°C and 280°C were 30 min, 30 min, 30 min and 120 min respectively. The heating rate was 5°C / min, and a pre-oxidized polyacrylonitrile nanofiber membrane was prepared.
[0115] The prepared pre-oxidized polyacrylonitrile nanofiber membrane was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at a preset carbonization temperature of 700°C for 10 min to prepare a polyacrylonitrile-based carbon nanofiber membrane.
[0116] Preparation of sulfonated polypropylene fiber and polypropylene-based carbon fiber:
[0117] The polypropylene fiber was prepared by a laboratory small melt spinning machine with a spinning temperature of 200°C and a take-up roller speed of 500-3000 r / min.
[0118] The prepared polyethylene fiber is placed in sulfuric acid for sulfonation at a sulfonation temperature of 130° C. for a sulfonation time of 180 min to prepare a sulfonated polypropylene fiber.
[0119] The prepared sulfonated polyethylene fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at a preset carbonization temperature of 500°C for 10 min to prepare polypropylene-based carbon fiber. Preparation of pre-oxidized lignin fiber and lignin-based carbon fiber:
[0120] The lignin fiber was prepared by a laboratory small melt spinning machine with a spinning temperature of 180°C and a take-up roller speed of 500 r / min-2500 r / min.
[0121] The prepared lignin fiber was placed in an oven for pre-oxidation, with the residence time at 210°C, 230°C, and 250°C being 30 min, 30 min, and 30 min, respectively, and the heating rate being 2°C / min, to prepare pre-oxidized lignin fiber.
[0122] The prepared pre-oxidized lignin fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at the preset carbonization temperature of 900°C for 10 min to prepare lignin-based carbon fiber. Preparation of pre-oxidized asphalt fiber and asphalt-based carbon fiber:
[0123] The asphalt fibers were prepared using a laboratory small melt spinning machine with a spinning temperature of 280°C and a take-up roller speed of 500-3000 r / min.
[0124] The prepared asphalt fiber was placed in an oven for pre-oxidation. The residence time at 230°C, 250°C and 280°C was 30 min, 30 min and 60 min respectively. The heating rate was 5°C / min, and pre-oxidized asphalt fiber was prepared.
[0125] The prepared pre-oxidized asphalt fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and kept at a preset carbonization temperature of 700°C for 10 min to prepare asphalt-based carbon fiber. Preparation of sulfonated polyethylene fiber and polyethylene-based carbon fiber:
[0126] The polyethylene fiber was prepared by a laboratory small melt spinning machine with a spinning temperature of 180°C and a take-up roller speed of 500-3000 r / min.
[0127] The prepared polyethylene fiber is placed in sulfuric acid for sulfonation at a sulfonation temperature of 120° C. and a sulfonation time of 180 min to prepare sulfonated polyethylene fiber.
[0128] The prepared sulfonated polyethylene fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at a preset carbonization temperature of 1000°C for 10 min to prepare polyethylene-based carbon fiber. Preparation of pre-oxidized viscose fiber and viscose-based carbon fiber:
[0129] The commercially available viscose fiber was placed in an oven for pre-oxidation. The residence times at 200°C, 230°C and 250°C were 30 min, 30 min and 30 min respectively. The heating rate was 5°C / min, and pre-oxidized viscose fiber was prepared.
[0130] The prepared pre-oxidized viscose fiber was placed in a tubular furnace for carbonization at a heating rate of 5°C / min and stayed at a preset carbonization temperature of 1000°C for 10 min to prepare viscose-based carbon fiber.
[0131] Preparation of element (cobalt, nickel or iron) doped polycarbosilane:
[0132] Using cobalt acetylacetonate (nickel acetylacetonate or iron acetylacetonate) as a metal element source and xylene as a solvent, polycarbosilane is dissolved in xylene in a three-necked flask, cobalt acetylacetonate (nickel acetylacetonate or iron acetylacetonate) is added for magnetic stirring, then the temperature is raised to 130°C for modification and cross-linking, and finally the solvent is removed to obtain element-doped polycarbosilane (the mass fraction of the doping element in the polycarbosilane is 10wt%), i.e., cobalt-doped polycarbosilane (nickel-doped polycarbosilane or iron-doped polycarbosilane).
[0133] Example 1
[0134] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0135] (a) 35 wt% of polyethylene particles, 20 wt% of polyisoprene particles, 20 wt% of polyacrylonitrile-based carbon fiber powder (with an average fiber length of 0.03 mm, an average fiber diameter of 8 μm, and a fiber carbonization temperature of 700°C), 10 wt% of polypropylene-based carbon fiber powder (with an average fiber length of 0.5 mm, an average fiber diameter of 10 μm, and a fiber carbonization temperature of 500°C), and 10 wt% of lignin-based carbon fiber (with an average fiber length of 5 mm, an average fiber diameter of 9 μm, and a fiber carbonization temperature of 500°C) were mixed. The mixture is prepared by mixing 100 wt % of 100 wt % of asphalt-based carbon fibers (with an average fiber length of 1 mm, an average fiber diameter of 6 μm, and a carbonization temperature of 900° C.) with a high-speed disperser, and then putting the mixture into an internal mixer for melt blending, the internal mixing temperature is 180° C., and the internal mixing time is 10 min, and then putting it into a crusher for crushing and granulation to obtain blended pellets; then putting the blended pellets into a twin-screw extruder for secondary blending, extrusion and granulation to obtain uniformly blended fiber-reinforced polyolefin (POCF) particles;
[0136] The POCF particles were pressed into a film using a hot press at a temperature of 180°C, a time of 5 min, and a pressure of 20 MPa to obtain a fiber-reinforced polyolefin (POCF) film (thickness of 20 μm).
[0137] (b) The fiber-reinforced polyolefin film was surface-modified using plasma (medium: air; discharge voltage: 75 V; treatment time: 5 min), and then the film was placed in concentrated sulfuric acid and sulfonated (cross-linked) using concentrated sulfuric acid at a sulfonation temperature of 120°C and a sulfonation time of 10 h to obtain an infusible intermediate (SPOCF).
[0138] (c) The infusible intermediate SPOCF is immersed in a carbon precursor solution (asphalt / carbon tetrachloride solution) for 15 minutes under vacuum, and then heat-stabilized in an oven at 300° C. for 5 hours to obtain a carburized film; wherein the mass fraction of asphalt in the carburized film is 20%.
[0139] (d) The carburized film is placed in a silicon-containing precursor solution (polycarbosilane / toluene solution) and vacuum-impregnated for 30 minutes, and then dried in an oven at 80° C. for 6 hours to obtain a carburized and siliconized product; wherein the mass fraction of polycarbosilane in the carburized and siliconized product is 50%.
[0140] (e) placing the carburized and siliconized product (carburized and siliconized film) in a pyrolysis furnace and performing pyrolysis treatment under the protection of a nitrogen atmosphere at a pyrolysis temperature of 1500° C. for a pyrolysis time of 120 min to obtain a carbon / carbon film (carbon / carbon film containing a SiC phase);
[0141] The carbon / carbon film after pyrolysis is subjected to a densification treatment, which includes immersing the carbon / carbon film in an asphalt / carbon tetrachloride solution and a polycarbosilane / toluene solution for carburizing and siliconizing treatment, and then pyrolyzing. The specific immersion conditions and pyrolysis process conditions are the same as those in steps (c), (d) and (e), respectively. The densification treatment is carried out three times to obtain a carbon / carbon composite material containing a SiC phase, namely a densified C / C-SiC film.
[0142] Example 2
[0143] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0144] (a) 0.5wt% polyacrylonitrile-based carbon nanofiber powder (average fiber length of 0.03mm, average fiber diameter of 500nm, fiber carbonization temperature of 700°C) and 99.5wt% polyethylene resin are blended by a high-speed disperser, and then the blended material is put into a mixer for melt blending at a mixer temperature of 180°C for 10min, and then put into a crusher for crushing and granulation to obtain blended pellets; then the blended pellets are put into a twin-screw extruder for secondary blending and extrusion granulation to obtain uniformly blended carbon nanofiber reinforced polyethylene particles (PECF). A melt spinning machine is used to prepare carbon nanofiber reinforced polyethylene fibers with an average diameter of 40μm.
[0145] (b) The carbon nanofiber reinforced polyethylene fiber is subjected to oxidative dehydrogenation by radiation irradiation (acceleration voltage: 1.5 MeV, beam current: 2 mA), and then the irradiated carbon nanofiber reinforced polyethylene fiber is placed in molten sulfur for vulcanization under a nitrogen atmosphere at a vulcanization temperature of 280°C and a vulcanization time of 5 hours. After the reaction is completed, the residual sulfur on the fiber surface is washed away with toluene, and then the fiber is vacuum dried in a vacuum oven to obtain an infusible intermediate, namely a vulcanized fiber intermediate.
[0146] (c) The vulcanized fiber intermediate is placed in a tubular furnace for a first pyrolysis (carbonization) treatment at a pyrolysis temperature of 3000° C. for 10 min to obtain a carbon / carbon material (carbonized polyethylene fiber).
[0147] (d) The carbon / carbon material is placed in an iron-doped polycarbosilane / toluene solution and vacuum impregnated for 5 minutes, and then vacuum dried in an oven at 50° C. for 20 hours to obtain a siliconized product (siliconized precursor fiber); wherein the mass fraction of iron-doped polycarbosilane in the siliconized precursor fiber is 20%.
[0148] (e) The siliconized precursor fiber is placed in a graphite furnace and subjected to a second pyrolysis treatment under the protection of an argon atmosphere. The pyrolysis temperature is 2650° C. and the pyrolysis time is 2 h to obtain a carbon / carbon composite material (C / C-SiC fiber).
[0149] Example 3
[0150] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0151] (a) 10 wt% of maleic anhydride grafted polyethylene particles, 20 wt% of polyisobutylene particles, 45 wt% of polypentene particles, 5 wt% of pre-oxidized lignin fiber powder (average fiber length of 10 mm, average fiber diameter of 5 μm), 10 wt% of pre-oxidized asphalt fiber powder (average fiber length of 2 mm, average fiber diameter of 8 μm), 10 wt% of polyimide-based carbon fiber (average fiber length of 3 mm, average fiber diameter of 10 μm, carbonization temperature of 1200°C) are blended together in a high-speed disperser, and then the blend is placed in an internal mixer for melt blending at a mixing temperature of 160°C and a mixing time of 15 min, and then placed in a crusher for crushing and granulation to obtain blended pellets; the blended pellets are then placed in a twin-screw extruder for secondary blending, extrusion and granulation to obtain uniformly blended fiber-reinforced polyolefin particles; and then an injection molding machine is used to process the obtained fiber-reinforced polyolefin particles into crucible components.
[0152] (b) The prepared crucible component is pre-crosslinked for 10 minutes using a sulfur trioxide / N2 mixed gas, and then placed in a blast oven for thermal oxidation at 270°C for 10 minutes to obtain an infusible intermediate, i.e., a cross-linked and stabilized crucible component.
[0153] (c) The cross-linked and stabilized crucible component is immersed in a carbon precursor solution (polyacrylonitrile / DMSO solution) for vacuum impregnation for 30 minutes, and then heat-stabilized in an oven at 300° C. for 7 hours to obtain a carburized product; wherein the mass fraction of polyacrylonitrile in the carburized product is 20%.
[0154] (d) The carburized product is placed in a silicon-containing precursor solution (n-tetramethylsilane solution) and vacuum impregnated for 40 minutes, and then dried in an oven at 200° C. for 6 hours to obtain a carburized and siliconized product; wherein the mass fraction of n-tetramethylsilane in the carburized and siliconized product is 50%.
[0155] (e) placing the carburized and siliconized product (the crucible component after carburization and siliconization) in a pyrolysis furnace and pyrolyzing it under the protection of an argon atmosphere at a pyrolysis temperature of 1500° C. for 180 min to obtain a carbon / carbon-silicon carbide crucible (C / C-SiC crucible);
[0156] The C / C-SiC crucible is subjected to a densification treatment, which includes immersing the C / C-SiC crucible in a polyacrylonitrile / DMSO solution and a tetramethylsilane solution, and then pyrolyzing the crucible. The specific immersion conditions and pyrolysis process conditions are the same as those in steps (c), (d) and (e), respectively. The densification treatment is performed 5 times in total to obtain a carbon / carbon composite material containing a SiC phase, namely a densified C / C-SiC crucible.
[0157] Example 4
[0158] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0159] (a) 20 wt% of carbon nanotube modified polypropylene particles, 20 wt% of poly-4-methyl-1-pentene particles, 10 wt% of poly-1-hexene particles, 5 wt% of poly-3-methylbutene-1 particles, 5 wt% of polybutadiene particles, 5 wt% of pre-oxidized polyacrylonitrile fiber powder (with an average fiber length of 30 mm and an average fiber diameter of 9 μm), 15 wt% of sulfonated polypropylene fiber powder (with an average fiber length of 3 mm and an average fiber diameter of 4 μm), 20 wt% of sulfonated polypropylene fiber powder (with an average fiber length of 3 mm and an average fiber diameter of 4 μm), and 10 wt% of poly-1-hexene particles were mixed. The fiber powder (the fiber length is 6 mm and the average fiber diameter is 15 μm) is blended together with the olefin fiber powder through a high-speed disperser, and then the blended material is put into an internal mixer for melt blending, the internal mixing temperature is 190° C., and the internal mixing time is 20 min. Then, it is put into a crusher for crushing and granulation to obtain blended pellets; the blended pellets are then put into a twin-screw extruder for secondary blending, extrusion and granulation to obtain uniformly blended fiber-reinforced polyolefin particles; and then a 3D particle printer is used to process the obtained fiber-reinforced polyolefin particles into cylindrical parts.
[0160] (b) The cylindrical part was brominated with liquid bromine for 18 h and then dried in a vacuum oven at 100° C. for 10 h to obtain an infusible intermediate, i.e., a cross-linked and stabilized cylindrical part.
[0161] (c) The cross-linked and stabilized cylindrical component is placed in a pyrolysis furnace and subjected to the first pyrolysis treatment under the protection of an argon atmosphere. The pyrolysis temperature is 700° C. and the pyrolysis time is 10 min to obtain a carbon / carbon material (carbonized 3D cylindrical component).
[0162] (d) The carbonized 3D cylindrical component is immersed in a carbon precursor solution (phenolic resin / hexamethylenetetramine / acetone solution) for vacuum impregnation for 180 minutes, and then heat stabilized in an oven at 150°C for 20 hours to obtain a carburized product (carburized 3D cylindrical component); wherein the mass fraction of phenolic resin in the carburized 3D cylindrical component is 60%, and hexamethylenetetramine is used as a curing agent for the phenolic resin, and its added amount is 10% of the mass of the phenolic resin.
[0163] (e) placing the carburized 3D cylindrical component in a pyrolysis furnace and performing a second pyrolysis treatment under nitrogen atmosphere protection, with a pyrolysis temperature of 500° C. and a pyrolysis time of 300 min to obtain a C / C 3D cylindrical component;
[0164] The C / C 3D cylindrical component is subjected to a densification treatment, which includes impregnating the C / C 3D cylindrical component in a phenolic resin / hexamethylenetetramine / acetone solution and then pyrolyzing it. The specific impregnation conditions and pyrolysis process conditions are the same as those in steps (d) and (e), respectively. The densification treatment is performed 9 times in total to obtain a carbon / carbon composite material, namely a densified C / C 3D cylindrical component.
[0165] Example 5
[0166] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0167] (a) 20 wt% of polyethylene particles, 30 wt% of polydicyclopentadiene particles, 10 wt% of polyethylene norbornene particles, 10 wt% of polyethylene-based norbornene particles, 10 wt% of pre-oxidized viscose fiber powder (with an average fiber length of 6 mm and an average fiber diameter of 20 μm) and 20 wt% of polyethylene-based carbon fiber (with an average fiber length of 30 mm, an average fiber diameter of 10 μm and a carbonization temperature of 1000° C.) are blended together by a high-speed disperser, and then The blended material is then placed in an internal mixer for melt blending at a mixing temperature of 170°C and a mixing time of 25 min, and then placed in a crusher for crushing and granulation to obtain blended pellets; the blended pellets are then placed in a twin-screw extruder for secondary blending and extrusion granulation to obtain uniformly blended fiber-reinforced polyolefin particles; a hot press is used to press them into a film at a hot pressing temperature of 180°C, a hot pressing time of 5 min, and a hot pressing pressure of 15 MPa to obtain a fiber-reinforced polyolefin film (thickness of 20 μm).
[0168] (b) The fiber-reinforced polyolefin film was subjected to ammoxidation treatment using 200 mL of 5 M ammonium hydroxide at a temperature of 260° C. for 10 min to obtain an infusible intermediate, i.e., a stabilized fiber-reinforced polyolefin film.
[0169] (c) The stabilized fiber-reinforced polyolefin film is placed in a tubular furnace and pyrolyzed under a nitrogen atmosphere at a pyrolysis temperature of 1600° C. for 20 min to obtain a carbon / carbon material (carbonized film).
[0170] (d) immersing the carbonized film in a phenolic resin / hexamethylenetetramine / acetone solution, vacuum impregnating for 5 min, and then heat stabilizing in an oven at 170° C. for 1 h to obtain a carburized product (carburized film), wherein the mass fraction of the phenolic resin in the carburized film is 10%, and hexamethylenetetramine is used as a curing agent for the phenolic resin, and its addition amount is 10% of the mass of the phenolic resin;
[0171] (e) The carburized film is then placed in a cobalt-doped polycarbosilane / toluene solution and vacuum impregnated for 50 minutes, and then dried in an oven at 200° C. for 1 hour to obtain a carburized and siliconized product (carburized and siliconized film), wherein the mass fraction of cobalt-doped polycarbosilane in the carburized and siliconized film is 10%.
[0172] (f) The carburized and siliconized products were placed in a pyrolysis furnace and pyrolyzed for the second time under the protection of a nitrogen atmosphere. The pyrolysis temperature was 2000° C. and the pyrolysis time was 10 min to obtain a carbon / carbon composite material (C / C-SiC film).
[0173] Example 6
[0174] This embodiment provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0175] (a) A continuous viscose-based carbon fiber reinforced polypropylene composite sheet (PP-CF) was prepared by vacuum hot pressing using 60 wt % polypropylene as a matrix resin and 40 wt % viscose-based carbon fiber (average fiber length 5 mm, average fiber diameter 7 μm, carbonization temperature 1000° C.) as a reinforcement. The length and width of the sheet were both 7 cm, and the thickness was 2 mm.
[0176] (b) subsequently placing the continuous viscose-based carbon fiber reinforced polypropylene composite sheet in concentrated sulfuric acid, and sulfonating and cross-linking the sheet using concentrated sulfuric acid, the sulfonation temperature is 140° C., the sulfonation time is 30 h, and an infusible intermediate SPP-CF is obtained;
[0177] (c) immersing the infusible intermediate SPP-CF in a pitch / carbon tetrachloride solution, vacuum impregnating for 30 minutes, and then heat stabilizing in an oven at 270° C. for 5 hours to obtain a carburized product; wherein the mass fraction of the pitch in the carburized product is 30%;
[0178] (d) The carburized product is placed in a nickel-doped polycarbosilane / toluene solution and vacuum impregnated for 180 minutes, and then dried in an oven at 80° C. for 20 hours to obtain a carburized and siliconized product; wherein the mass fraction of the nickel-doped polycarbosilane in the carburized and siliconized product is 50%.
[0179] (e) The carburized and siliconized products are placed in a pyrolysis furnace and pyrolyzed under a nitrogen atmosphere at a pyrolysis temperature of 1600° C. for 150 min to obtain a carbon / carbon composite material containing a SiC phase (i.e., a C / C-SiC sheet).
[0180] Comparative Example 1
[0181] This comparative example provides a method for preparing a carbon / carbon composite material (i.e., a C / C film). Except that step (d) siliconization treatment is not performed and step (d) siliconization treatment is not performed in the subsequent densification process, the remaining steps and process parameters are the same as those in Example 1.
[0182] Comparative Example 2
[0183] This comparative example provides a method for preparing a carbon / carbon composite material (i.e., C / C film), except that step (b) is not performed, and the fiber-reinforced polyolefin film obtained in step (a) is directly subjected to step (c) carburization treatment. The remaining steps and process parameters are the same as those in Example 1.
[0184] However, during the process of step (e), the carburized and siliconized product (carburized and siliconized film) was placed in a pyrolysis furnace and pyrolyzed under the protection of a nitrogen atmosphere. The pyrolysis temperature was 1500°C and the pyrolysis time was 120 min. After the pyrolysis treatment, it was found that the polyolefin matrix in the carburized and siliconized product was completely pyrolyzed into small molecular gases and could not be carbonized to obtain a sample. Therefore, subsequent densification treatment could not be carried out, and thus a carbon / carbon composite material could not be obtained.
[0185] Comparative Example 3
[0186] This comparative example provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0187] (a) 50% of polyethylene particles and 50% of polyisoprene particles are blended by a high-speed disperser, and then the blended pellets are placed in a mixer for melt blending at a mixer temperature of 180°C and a mixer time of 10 minutes, and then placed in a crusher for crushing and granulation. Subsequently, the blended pellets are placed in a twin-screw extruder for secondary blending, extrusion and granulation to obtain uniformly blended polyolefin particles. The polyolefin particles are pressed into a film by a hot press at a hot pressing temperature of 180°C, a hot pressing time of 5 minutes, and a hot pressing pressure of 20 MPa to obtain a polyolefin film (thickness of 20 μm).
[0188] (b) The film is surface modified by plasma (medium: air; discharge voltage: 75 V; treatment time: 5 min), and then placed in concentrated sulfuric acid. The polyolefin film is sulfonated and cross-linked by concentrated sulfuric acid at a sulfonation temperature of 120° C. for 10 h to obtain a sulfonated polyolefin film.
[0189] (c) The sulfonated polyolefin film is placed in a pyrolysis furnace and pyrolyzed under a nitrogen atmosphere at a pyrolysis temperature of 1500° C. for 120 min to obtain a carbon film.
[0190] Comparative Example 4
[0191] This comparative example provides a method for preparing a carbon / carbon composite material, comprising the following steps:
[0192] (a) 10 wt% of maleic anhydride grafted polyethylene particles, 20 wt% of polyisobutylene particles, 45 wt% of polypentene particles, 5 wt% of pre-oxidized lignin fiber powder (average fiber length of 10 mm, average fiber diameter of 5 μm), 10 wt% of pre-oxidized asphalt fiber powder (average fiber length of 2 mm, average fiber diameter of 8 μm), 10 wt% of polyimide-based carbon fiber (average fiber length of 3 mm, average fiber diameter of 10 μm, carbonization temperature of 1200°C) are blended together in a high-speed disperser, and then the blend is placed in an internal mixer for melt blending at a mixing temperature of 160°C and a mixing time of 15 min, and then placed in a crusher for crushing and granulation to obtain blended pellets; the blended pellets are then placed in a twin-screw extruder for secondary blending, extrusion and granulation to obtain uniformly blended fiber-reinforced polyolefin particles; and then an injection molding machine is used to process the obtained fiber-reinforced polyolefin particles into crucible components.
[0193] (b) The prepared crucible component is pre-crosslinked for 10 minutes using a sulfur trioxide / N2 mixed gas, and then placed in a blast oven for thermal oxidation at 270°C for 10 minutes to obtain an infusible intermediate, i.e., a cross-linked and stabilized crucible component.
[0194] (c) placing the cross-linked and stabilized crucible component into a pyrolysis furnace and performing pyrolysis under the protection of an argon atmosphere at a pyrolysis temperature of 1500° C. for 180 min to obtain a carbon / carbon composite material (C / C crucible).
[0195] Comparative Example 5
[0196] This comparative example provides a method for preparing a carbon / carbon ceramic-based composite material. Except that the fiber reinforcement in step (a) is changed to T300 carbon fiber (average fiber length 6 mm, average fiber diameter 7 μm, preparation temperature >1300°C), the remaining steps and process parameters are the same as those in Example 1.
[0197] In order to compare the technical effects of the above embodiments and comparative examples, the following experimental examples are specially designed.
[0198] Experimental Example 1
[0199] Taking Example 1, Comparative Example 1 and Comparative Example 3 as examples, the morphologies of the C / C-SiC film prepared in Example 1 and the carbon films prepared in Comparative Example 1 and Comparative Example 3 were detected. Figure 1 As shown. Among them, Figure 1 (a) is comparative example 3, Figure 1 (b) is Comparative Example 1, Figure 1 (c) is Example 1. By comparison, it can be found that when only polyolefin is used as the precursor in Comparative Example 3 (without adding cyclized organic fiber), the carbon film obtained after sulfonation-carbonization is brittle and breaks during the thermal stabilization and carbonization process, and a complete carbon film with certain mechanical properties cannot be obtained. When the polyolefin composite material with cyclized organic fiber as the reinforcement is used as the precursor, the fiber reinforcement plays a supporting role, and the prepared C / C film can be bent to a certain extent and has good flexibility (Comparative Example 1). Compared with Comparative Examples 1 and 3, the C / C-SiC film prepared in Example 1 can be folded to a greater extent, indicating that the introduction of the SiC phase further improves the mechanical properties of the film.
[0200] Experimental Example 2
[0201] The properties of the composite materials prepared in each embodiment and comparative example were tested, and the specific results are shown in Table 2. The test methods for apparent porosity and volume density are based on GB / T 25995-2010; the anti-oxidation performance of the composite material was tested by a static oxidation method, the composite material was placed in a muffle furnace at 800°C for 20 hours, and the mass retention rate was calculated based on the mass of the sample before and after heating; the test method for minimum reflection loss was based on JC / T 2499-2018.
[0202] Table 2
[0203]
[0204] Note: “ / ” in the table means that the relevant experimental data cannot be determined.
[0205] From the data in Table 2 above, it can be seen that the C / C composite material containing SiC phase prepared by carburizing and siliconizing with cyclized organic fiber as reinforcement has significantly improved structural density and oxidation resistance compared with pure carbon material, and at the same time has excellent microwave absorption performance, which proves that high-performance C / C composite material containing SiC phase with microwave absorption performance can be prepared using polyolefin as precursor.
[0206] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention are within the scope of protection of the pending claims of the present invention.
Claims
1. A method for preparing a carbon / carbon composite material, It is characterized in that The following steps are involved: (a) using polyolefin as a matrix resin and cyclized organic fiber as a reinforcement to prepare a carbon / carbon composite material precursor; wherein the polyolefin is a polyolefin that can be carbonized after chemical crosslinking and pyrolysis treatment; (b) chemically cross-linking the carbon / carbon composite material precursor to obtain an infusible intermediate; (c) subjecting the infusible intermediate to a first pyrolysis treatment to obtain a carbon / carbon material; (d) subjecting the infusible intermediate of step (b) or the carbon / carbon material of step (c) to carburizing and / or siliconizing to obtain an infiltration product; (e) subjecting the infiltration product to a second pyrolysis treatment and an optional densification treatment to obtain a carbon / carbon composite material; The preparation temperature of the cyclized organic fiber in step (a) is lower than the pyrolysis temperature of the first pyrolysis treatment in step (c) and the pyrolysis temperature of the second pyrolysis treatment in step (e).
2. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that In step (a), the polyolefin includes polyethylene, polypropylene, polybutene, polyisobutylene, polypentene, poly-4-methyl-1-pentene, poly-1-hexene, poly-3-methylbutene-1, polybutadiene, polyisoprene, polydicyclopentadiene, polyethylene norbornene, polyvinyl norbornene homopolymers and grafted modified products thereof or carbon nanofiller modified products thereof, or binary, ternary, or multi-component copolymers containing the above homopolymer structural units and grafted modified products thereof or carbon nanofiller modified products thereof or one or more thereof; Preferably, the graft-modified product of the polyolefin homopolymer or copolymer is a modified product obtained by graft-modifying the polyolefin homopolymer or copolymer with a polar monomer, and the polar monomer includes at least one of maleic anhydride, acrylic acid, α-methacrylic acid, acrylamide, glycidyl methacrylate or styrene; Preferably, the carbon nanofiller-modified product of the polyolefin homopolymer or copolymer is a modified product of the polyolefin homopolymer or copolymer modified with a carbon nanofiller, and the carbon nanofiller includes at least one of carbon nanotubes, alkyl-modified carbon nanotubes, siloxane-modified carbon nanotubes, graphene nanosheets, alkyl-modified graphene nanosheets, graphene oxide or graphite.
3. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that The cyclized organic fiber includes one or more of polyacrylonitrile-based carbon fiber, preoxidized polyacrylonitrile fiber, asphalt-based carbon fiber, preoxidized asphalt fiber, viscose-based carbon fiber, preoxidized viscose fiber, lignin-based carbon fiber, preoxidized lignin fiber, polyimide-based carbon fiber, polyimide fiber, polyethylene-based carbon fiber, sulfonated polyethylene fiber, polypropylene-based carbon fiber or sulfonated polypropylene fiber; Preferably, the carbonization temperature of the polyacrylonitrile-based carbon fiber, asphalt-based carbon fiber, viscose-based carbon fiber, lignin-based carbon fiber, polyimide-based carbon fiber, polyethylene-based carbon fiber and polypropylene-based carbon fiber is 400-1200°C, preferably 400-900°C.
4. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that The cyclized organic fibers are in the form of chopped fibers and / or continuous fibers, wherein the chopped fibers have a length of 0.03-30 mm; And / or, the mass ratio of the cyclized organic fiber to the polyolefin is (0.1-90):
100.
5. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that In step (b), the chemical cross-linking treatment includes one or more of sulfonation treatment, thermal oxidation treatment, ammonia oxidation treatment, bromination treatment, plasma treatment, irradiation treatment or sulfurization treatment; And / or, in step (c), the pyrolysis temperature of the first pyrolysis treatment is 700-3000° C., the pyrolysis time is 10-180 min, and the pyrolysis is carried out in a protective atmosphere.
6. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that In step (d), the infusible intermediate or the carbon / carbon material is immersed in a carbon precursor solution for carburizing treatment and / or immersed in a silicon-containing precursor solution for siliconizing treatment; Preferably, the carbon precursor in the carbon precursor solution includes one or more of asphalt, lignin, polyacrylonitrile or phenolic resin; Preferably, the solvent in the carbon precursor solution includes one or more of carbon tetrachloride, toluene, dimethyl sulfoxide or acetone; Preferably, the carbon precursor accounts for 0-60% of the total mass of the infiltration product obtained after carburizing treatment; Preferably, the specific steps of the carburizing treatment include: immersing the infusible intermediate or carbon / carbon material in a carbon precursor solution for 5-180 minutes, and then performing a thermal stabilization treatment at 50-300° C. for 1-20 hours.
7. The method for preparing the carbon / carbon composite material according to claim 6, It is characterized in that In step (d), the silicon-containing precursor in the silicon-containing precursor solution includes one or more of n-tetramethylsilane, polycarbosilane or element-doped polycarbosilane, wherein the element doped in the element-doped polycarbosilane includes at least one of boron, titanium, aluminum, iron, cobalt, nickel or zirconium; and / or, the silicon-containing precursor accounts for 0-50% of the total mass of the infiltration product obtained after siliconizing treatment; And / or, the specific steps of the siliconizing treatment include: immersing the infusible intermediate or the carbon / carbon material or the infiltration product obtained after the carburizing treatment in a silicon-containing precursor solution for 5-180 minutes, and then drying at 50-200° C. for 1-20 hours.
8. The method for preparing the carbon / carbon composite material according to claim 1, It is characterized in that In step (e), the pyrolysis temperature of the second pyrolysis treatment is 500-2650° C., the pyrolysis time is 0.1-5 h, and the pyrolysis is carried out in a protective atmosphere; and / or, in step (e), the densification treatment includes the step of impregnating the pyrolysis product obtained after the second pyrolysis treatment in the carbon precursor solution and / or the silicon-containing precursor solution in step (d), and then pyrolyzing it again; And / or, the densification treatment is performed 0-10 times.
9. A carbon / carbon composite material, It is characterized in that The carbon / carbon composite material is prepared by the preparation method of any one of claims 1 to 8.
10. A method for preparing the carbon / carbon composite material according to any one of claims 1 to 8 or use of the carbon / carbon composite material according to claim 9 in the fields of aerospace, automobile manufacturing or energy.
Citation Information
Patent Citations
C / C-SiC composite material of sandwich structure and preparation method thereof
CN107879758A
Preparation method of polyimide resin carbon modified C / C-SiC friction material
CN114645449A
Precusor conversion preparation method of carbon fibre reinforced silicon carbide composite material
CN101717255A
Preparation method of C / C-SiC composite material
CN103708846A
A process for making a stabilized fabricated article from polyolefin
CN106170587A
Cited By
In-situ ceramicized EPDM erosion-resistant thermal insulation material and preparation method thereof
CN119752051A