Two-step aluminum oxide ceramic connecting method based on aluminum oxide powder solder sintering and glass permeation principle

Through the two-step connection method of alumina powder sintering and glass penetration, the problems of joint thermal expansion coefficient differences and pore defects in traditional glass welding methods are solved, and ceramic connections with high strength, high temperature resistance and thermal shock resistance are achieved.

CN118754698AActive Publication Date: 2024-10-11CHANGCHUN UNIV OF TECH

Patent Information

Application Number
CN202411015868.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-10-11
Estimated Expiration
2044-07-26

AI Technical Summary

Technical Problem

The traditional glass welding method results in a large difference in thermal expansion coefficient between the ceramic joint and the base material, insufficient thermal shock resistance and high temperature resistance. When improving high temperature resistance, the fluidity of the solder decreases, resulting in the formation of pore defects, which limits the application of the connection.

Method used

A two-step connection method of alumina powder sintering and glass penetration is adopted. The porous joint is first formed by alumina powder, and then filled with glass solder penetration to eliminate weld holes and improve the density and high temperature resistance of the joint.

Benefits of technology

The strength, thermal shock resistance and high temperature resistance of the joint are significantly improved. The thermal expansion coefficient of the weld is close to that of the base material. The bending strength of the weld reaches more than 90% at 1000°C, and the strength remains stable after 100 thermal shock cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118754698A_ABST
    Figure CN118754698A_ABST
Patent Text Reader

Abstract

The invention discloses a two-step aluminum oxide ceramic connecting method based on an aluminum oxide powder solder sintering and glass permeation principle, and belongs to the technical field of welding. The method comprises the following steps: firstly, connecting aluminum oxide ceramics by adopting aluminum oxide powder; and then penetrating and filling holes (including open holes and closed holes) in the weld joint by using glass solder so as to obtain a compact weld joint layer. The content of Al2O3 phase in the obtained aluminum oxide / aluminum oxide joint welding seam is higher than 50%, and the difference between the thermal expansion coefficient of the welding seam and the thermal expansion coefficient of base metal is smaller than 2%. The joint has excellent mechanical properties, high temperature resistance and thermal shock resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of welding, and in particular to a two-step method for connecting alumina ceramics based on the principles of alumina powder solder sintering and glass penetration. Background Art

[0002] Alumina ceramics have many advantages such as high hardness, high strength, high toughness, good corrosion resistance, etc., and are widely used in machinery, chemical industry, aerospace and other fields. However, due to the inherent brittleness and difficulty in mechanical processing of ceramic materials, in order to construct ceramic parts with complex shapes and large sizes, connection technology is often required.

[0003] Among the various methods of connecting ceramic materials, glass solder is more suitable for connecting ceramics because of the good chemical compatibility between glass solder and ceramics. However, the principle of traditional glass connection method is similar to brazing, and the microstructure and physical and chemical properties of the weld are quite different from those of the parent material. For example, the thermal expansion coefficient, elastic modulus, softening temperature, etc. of the weld are quite different from those of the ceramic parent material, which leads to insufficient thermal shock resistance and high temperature resistance of the joint. Adding a high melting point second phase to glass solder is an effective method to improve the high temperature resistance of the joint. In particular, adding powder with the same chemical composition as the parent material as the second phase to the solder can not only improve the high temperature resistance of the joint, but also reduce the difference in thermal expansion coefficient between the parent material and the weld. However, the introduction of a high melting point phase into the solder will inevitably lead to a decrease in the fluidity of the solder, thereby leading to the formation of pore defects, which limits the application of this method. Summary of the invention

[0004] The purpose of the present invention is to provide a two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass penetration, so as to obtain welds with high Al2O3 content, eliminate weld hole defects, and thus improve joint strength, thermal shock resistance and high temperature resistance.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration. The method first uses Al2O3 powder to connect alumina ceramics to obtain an "alumina / porous Al2O3 / alumina" joint; then uses glass solder to infiltrate and fill the "alumina / porous Al2O3 / alumina" joint to obtain an "alumina / Al2O3+microcrystalline glass / alumina" joint, thereby achieving a dense connection of the alumina ceramics.

[0007] The particle size of the Al2O3 powder is 20-100nm.

[0008] The composition of the glass solder is calculated by weight percentage as follows: Al2O3: 15-25%, RE2O3: 50-60%, B2O3: 1-5%, SiO2: 15%-25%, ZrO2: 1-5%, TiO2: 1-5%; wherein RE2O3 is one or more of La2O3, Y2O3, Dy2O3 and Ho2O3.

[0009] The method specifically comprises the following steps:

[0010] (1) Material preparation: After grinding and polishing the surface of the alumina ceramic to be welded, ultrasonic cleaning is performed with acetone as the medium for 5-20 minutes, and then blown dry for later use;

[0011] (2) Preparation of glass solder: weighing various oxide raw materials according to the composition of the glass solder, uniformly mixing them, and preparing glass solder powder by a melting-water quenching method;

[0012] (3) First step of connection: Al2O3 powder is mixed with anhydrous ethanol to prepare slurry I, and slurry I is evenly coated on the surface of the alumina ceramic to be welded, and the two surfaces to be welded coated with slurry I are tightly fitted, and after drying, a "alumina ceramic / Al2O3 powder / alumina ceramic" sandwich assembly structure is constructed. The sandwich assembly structure is placed in a muffle furnace with air atmosphere and quickly heated to the welding temperature, and kept warm for a long enough time. After the insulation is completed, it is cooled to room temperature with the furnace to obtain an "alumina / porous Al2O3 / alumina" joint; no pressure is used during the connection process;

[0013] (4) Second step of infiltration: the glass solder powder prepared in step (2) is mixed with anhydrous ethanol to form slurry II, and slurry II is evenly applied to the surface of the joint connected in step (3); after drying, the slurry is placed in a muffle furnace with air atmosphere and quickly heated to the infiltration temperature, and kept warm for a long enough time to ensure that the glass solder completely penetrates and fills the weld. After the insulation is completed, the slurry is uniformly cooled to room temperature to obtain an "alumina / Al2O3+microcrystalline glass / alumina" joint.

[0014] In the above step (1), the grinding and polishing process is: grinding with 400#, 800#, and 1200# sandpaper in sequence, and then polishing with diamond polishing paste with particle sizes of 2.5μm, 1.5μm, and 0.5μm in sequence.

[0015] In the above step (2), the process of preparing glass solder powder by the melt-water quenching method is as follows: weighing the oxide raw material powder into a polytetrafluoroethylene ball mill, using alcohol as the ball milling medium and ZrO2 as the grinding balls for ball milling, the ball milling speed is 400-500 rpm, and the ball milling time is 2-5h; drying is performed after the ball milling is completed, and the dried material is poured into a platinum crucible, and placed in a muffle furnace with an air atmosphere and heated to 1500-1600°C. After keeping warm for 1-3h, the obtained glass melt is poured into deionized water to obtain glass fragments; the glass fragments are placed in an agate ball mill, using agate as the grinding balls for ball milling, the ball milling speed is 400-500 rpm, and the ball milling time is 2-5h. After the ball milling is completed, drying is performed, and the glass solder powder is obtained by sieving through a 200-mesh sieve for standby use.

[0016] When preparing slurry I in the above step (3), the mass of the added ethanol accounts for 40%-60% of the total mass of slurry I.

[0017] In the above step (3), after the sandwich assembly structure is placed in a muffle furnace, it is heated to a welding temperature of 1550-1650°C at a heating rate of 5-10°C / min, and kept warm for 20-30 minutes. After the insulation is completed, it is cooled to room temperature with the furnace for use.

[0018] When preparing slurry II in the above step (4), the mass of the added ethanol accounts for 40%-60% of the total mass of slurry II.

[0019] In the above step (4), the joint coated with slurry II is dried and placed in a muffle furnace, and then heated to a penetration temperature of 1450-1500°C at a heating rate of 5-10°C / min, and kept warm for 60-120 minutes. During the cooling process, the cooling rate is 2-10°C / min.

[0020] The design mechanism and beneficial effects of the present invention are as follows:

[0021] 1. The method of the present invention first connects alumina ceramics using alumina powder through the sintering principle. Then, using the principle of liquid glass penetrating between dense ceramic crystals, glass solder is used to infiltrate and fill the alumina / porous Al2O3 / alumina joint to eliminate weld defects, reduce thermal expansion differences, and improve the high temperature resistance and thermal shock resistance of the joint, and finally obtain a high-strength joint.

[0022] 2. The glass solder used in the present invention has excellent intergranular penetration ability, which can not only fill the through holes in the Al2O3 weld layer, but also fill the closed pore defects, and finally obtain a dense and defect-free alumina / alumina joint.

[0023] 3. The present invention can finally obtain a weld with an Al2O3 content higher than 50%, significantly reducing the difference in thermal expansion coefficient between the weld and the base material. The difference in thermal expansion coefficient between the weld and the ceramic base material is no more than 2%. After 100 room temperature-1000℃ thermal shock cycles, the joint strength does not decrease significantly.

[0024] 4. The present invention can obtain a weld composed of Al2O3 and a crystallized phase, which significantly improves the high temperature resistance of the joint. The bending strength of the joint at 1000°C can reach more than 90% of that of the alumina parent material. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a schematic diagram of the two-step welding process.

[0026] Figure 2 This is a microstructure photograph of the alumina ceramic joint obtained in Example 1.

[0027] Figure 3 This is a microstructure photograph of the alumina ceramic joint obtained in Comparative Example 1. DETAILED DESCRIPTION

[0028] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0029] Example 1

[0030] This embodiment is a two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass penetration. The welding process is as follows Figure 1 As shown, the specific steps include:

[0031] (1) Material preparation: Use 400#, 800#, and 1200# sandpaper to grind the surface of the alumina ceramic to be welded, and then use diamond polishing paste with a particle size of 2.5μm, 1.5μm, and 0.5μm to polish the surface of the ceramic to be welded. The polished alumina ceramic is ultrasonically cleaned with acetone as the medium for 20 minutes, and then blown dry for use.

[0032] (2) Preparation of glass solder: The composition of the glass solder used is (wt.%): Al2O3: 15%, Dy2O3: 55%, B2O3: 2%, SiO2: 22%, ZrO2: 3%, TiO2: 3%. Weigh the oxide powder raw materials according to the above proportions, and put them into a polytetrafluoroethylene ball mill with alcohol as the ball milling medium and ZrO2 as the grinding ball for ball milling. The ball milling speed is 450 rpm and the ball milling time is 4 hours. After ball milling, dry it in a vacuum drying oven at 70°C for 2 hours. Pour the dried raw materials into a platinum crucible and heat it to 1550°C in a muffle furnace. After keeping warm for 2 hours, pour the glass melt into deionized water to obtain glass fragments. Put the glass fragments into an agate ball mill for ball milling. The ball milling speed is 500 rpm and the ball milling time is 4 hours. After ball milling, dry it and pass it through a 200-mesh sieve to obtain the glass solder powder for use.

[0033] (3) The first step of connection: Al2O3 powder and anhydrous ethanol are mixed in a mass ratio of 1:1 to prepare slurry I, and slurry I is evenly applied to the surface of the alumina ceramic to be welded, and the two surfaces to be welded are tightly fitted, and after drying, a "alumina ceramic / Al2O3 powder / alumina ceramic" sandwich assembly structure is constructed. The sandwich assembly structure is placed in a muffle furnace with an air atmosphere and heated to 1550°C at a heating rate of 8°C / min, and kept warm for 30 minutes. After the insulation is completed, the joint is cooled to room temperature with the furnace. No pressure is used during the connection process;

[0034] (4) Second step of penetration: The glass solder powder prepared in step (2) is mixed with anhydrous ethanol in a mass ratio of 1:1 to form slurry II, and slurry II is evenly applied to the surface of the joint connected in step (2). After drying, it is placed in a muffle furnace with air atmosphere and rapidly heated to 1450°C at a heating rate of 8°C / min, and kept warm for 120 minutes to ensure that the glass solder completely penetrates and fills the joint weld. After the insulation is completed, the joint is cooled to room temperature at a rate of 5°C / min.

[0035] Figure 2 The microstructure photo of the alumina ceramic joint obtained in Example 1. By using glass solder for infiltration filling, the entire weld becomes complete and defect-free. At the same time, due to the slow cooling rate, the glass phase in the weld can be fully crystallized. In general, the distribution of each phase in the weld is relatively uniform. By using image analysis software, it is confirmed that Al2O3, crystalline phase Dy2Si2O7 and residual glass phase in this embodiment account for approximately 52.7%, 47.2% and 0.1% of the mass of the entire composite weld, respectively. It can be calculated by the mixing rule that the thermal expansion coefficient of the weld in this embodiment is 7.89×10 -6 / ℃, the difference from the parent material is only 2%. The room temperature bending strength of the "alumina / Al2O3+microcrystalline glass / alumina" joint prepared in Example 1 can reach 322MPa, which is basically the same as that of general commercial alumina ceramics. The bending strength at 1000℃ can reach 145MPa, reaching more than 90% of the alumina parent material under the same conditions. After 100 thermal shock cycles at room temperature-1000℃, the joint still maintains a strength of 320MPa, which is equivalent to the room temperature strength.

[0036] Example 2

[0037] The difference from Example 1 is that the heating time in step (3) is changed to 25 minutes, and the other steps are the same as Example 1. The room temperature bending strength of the joint obtained in this example is 308 MPa. The bending strength at 1000°C is 135 MPa. After 100 thermal shock cycles at room temperature-1000°C, the joint strength does not decrease significantly.

[0038] Example 3

[0039] The difference from Example 1 is that the connection temperature in step (3) is changed to 1600°C, and the other steps are the same as Example 1. The room temperature bending strength of the joint obtained in this example is 315MPa. The bending strength at 1000°C is 138MPa. After 100 thermal shock cycles at room temperature-1000°C, the joint strength does not decrease significantly.

[0040] Example 4

[0041] The difference from Example 1 is that the heating time in step (4) is changed to 60 minutes, and the other steps are the same as Example 1. The room temperature bending strength of the joint obtained in this example is 318 MPa. The bending strength at 1000°C is 140 MPa. After 100 thermal shock cycles at room temperature-1000°C, the joint strength does not decrease significantly.

[0042] Example 5

[0043] The difference from Example 1 is that the infiltration temperature in step (4) is changed to 1500°C, and the other steps are the same as Example 1. The room temperature bending strength of the joint obtained in this example is 311 MPa. The bending strength at 1000°C is 141 MPa. After 100 thermal shock cycles at room temperature-1000°C, the joint strength does not decrease significantly.

[0044] Example 6

[0045] The difference from Example 1 is that in step (2), Dy2O3 in the glass solder composition is replaced by La2O3 of equal mass, and the other steps are the same as Example 1. The crystals precipitated in the joint weld obtained in this example are mainly La2Si2O7. The room temperature bending strength of the joint is 303MPa. The bending strength at 1000℃ is 133MPa. After 100 thermal shock cycles at room temperature-1000℃, the joint strength does not decrease significantly.

[0046] Example 7

[0047] The difference from Example 1 is that in step (2), Dy2O3 in the glass solder composition is replaced by an equal amount of Y2O3, and the other steps are the same as Example 1. The crystals precipitated in the joint weld obtained in this example are mainly Y2Si2O7. The room temperature bending strength of the joint is 315MPa. The bending strength at 1000°C is 134MPa. After 100 thermal shock cycles at room temperature-1000°C, the joint strength does not decrease significantly.

[0048] Comparative Example 1

[0049] This comparative example uses a mixed solder of Al2O3 and glass solder in a weight ratio of 1:1 to connect alumina ceramics. The material preparation in step (1) and the glass solder preparation in step (2) are the same as those in Example 1.

[0050] Step (3) Joint connection: Al2O3 powder and glass solder powder of equal weight are mixed to obtain a mixed solder; the mixed solder is then mixed with anhydrous ethanol in a mass ratio of 1:1 to prepare a slurry, the slurry is evenly coated on the surface of the alumina ceramic to be welded, and a "sandwich" assembly structure is constructed after drying. The assembled joint is placed in a muffle furnace in an air atmosphere and quickly heated to 1550°C and kept warm for 120 minutes. After the insulation is completed, the joint is cooled to room temperature with the furnace.

[0051] No pressure is used during the connection process;

[0052] Figure 3 The microstructure photograph of the alumina joint obtained in Comparative Example 1. Since the introduction of high melting point Al2O3 powder reduces the wettability of the mixed solder on the surface of alumina ceramics, a large number of pore defects exist in the joint obtained by using Al2O3 / glass mixed solder.

[0053] Comparative Example 2

[0054] The difference from Example 1 is that the cooling rate in step (4) is changed to 50°C / min, and the other steps are the same as Example 1. The room temperature bending strength of the joint obtained in this example is 312MPa. However, due to the use of a faster cooling rate, the glass phase content in the weld is relatively high, and the bending strength at 1000°C is only 32MPa.

[0055] The mechanical properties of the joints obtained in the above Examples 1-7 and Comparative Examples 1-2 are shown in Table 1. As can be seen from the table, Examples 1-7 all achieved excellent room temperature strength, high temperature strength and strength after thermal shock cycles. Comparative Example 1 had the lowest room temperature strength of the joint due to the failure to form an effective connection. Comparative Example 2 had a lower high temperature strength due to the high glass phase content in the weld.

[0056] Table 1 Joint bending strength data of the embodiment and the comparative example

[0057]

Claims

1. A two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration, characterized in that: The method first uses Al2O3 powder to pre-connect alumina ceramics to obtain an "alumina / porous Al2O3 / alumina" joint; then uses glass solder to infiltrate and fill the "alumina / porous Al2O3 / alumina" joint to achieve a dense connection of the alumina ceramics.

2. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 1 is characterized in that: The particle size of the Al2O3 powder is 20-100nm; the composition of the glass solder is calculated by weight percentage: Al2O3: 15-25%, RE2O3: 50-60%, B2O3: 1-5%, SiO2: 15%-25%, ZrO2: 1-5%, TiO2: 1-5%.

3. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 2 is characterized in that: In the glass solder composition, RE2O3 is one or more of La2O3, Y2O3, Dy2O3 and Ho2O3.

4. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 2 is characterized in that: The method specifically comprises the following steps: (1) Material preparation: After grinding and polishing the surface of the alumina ceramic to be welded, ultrasonic cleaning is performed with acetone as the medium for 5-20 minutes, and then blown dry for later use; (2) Preparation of glass solder: weighing various oxide raw materials according to the composition of the glass solder, uniformly mixing them, and preparing glass solder powder by a melting-water quenching method; (3) First step of connection: Al2O3 powder is mixed with anhydrous ethanol to prepare slurry I, and slurry I is evenly coated on the surface of alumina ceramic to be welded, and the two surfaces to be welded are tightly fitted, and after drying, an "alumina ceramic / Al2O3 powder / alumina ceramic" sandwich assembly structure is constructed; the sandwich assembly structure is placed in a muffle furnace and quickly heated to the welding temperature in an air atmosphere, and kept warm for a sufficiently long time. After the insulation is completed, it is cooled to room temperature with the furnace to obtain an "alumina / porous Al2O3 / alumina" joint; no pressure is used during the connection process; (4) Second step of penetration: the glass solder powder prepared in step (2) is mixed with anhydrous ethanol to form slurry II, and slurry II is evenly applied to the surface of the joint connected in step (3); after drying, the slurry is placed in a muffle furnace and heated to the penetration temperature in an air atmosphere, and the temperature is kept for a sufficiently long time to ensure that the glass solder completely penetrates and fills the weld. After the insulation is completed, the joint is uniformly cooled to room temperature.

5. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 4 is characterized in that: In step (1), the grinding and polishing process is: grinding with 400#, 800#, and 1200# sandpaper in sequence, and then polishing with diamond polishing paste with particle sizes of 2.5μm, 1.5μm, and 0.5μm in sequence.

6. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 4 is characterized in that: In step (2), the process of preparing glass solder powder by the melt-water quenching method is as follows: weighing the oxide raw material powder into a polytetrafluoroethylene ball mill, using alcohol as the ball milling medium and ZrO2 as the grinding ball for ball milling, the ball milling speed is 400-500 rpm, and the ball milling time is 2-5h; drying is performed after the ball milling is completed, and the dried material is poured into a platinum crucible, and placed in a muffle furnace with an air atmosphere and heated to 1500-1600°C. After keeping warm for 1-3h, the obtained glass melt is poured into deionized water to obtain glass fragments; the glass fragments are placed in an agate ball mill, using agate as the grinding ball for ball milling, the ball milling speed is 400-500 rpm, and the ball milling time is 2-5h. After the ball milling is completed, drying is performed, and the glass solder powder is obtained through a 200-mesh sieve for standby use.

7. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 3 is characterized in that: When preparing slurry I in step (3), the mass of the added ethanol accounts for 40%-60% of the total mass of slurry I.

8. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 3 is characterized in that: In step (3), the sandwich assembly structure is placed in a muffle furnace, heated to a welding temperature of 1550-1650°C at a heating rate of 5-10°C / min, and kept warm for 20-30 minutes. After the insulation is completed, it is cooled to room temperature with the furnace.

9. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 3 is characterized in that: When preparing slurry II in step (4), the mass of the added ethanol accounts for 40%-60% of the total mass of slurry II.

10. The two-step method for connecting alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration according to claim 3, characterized in that: In step (4), the joint coated with slurry II is dried and placed in a muffle furnace, and then heated to a penetration temperature of 1450-1500°C at a heating rate of 5-10°C / min, and kept warm for 60-120 minutes. The cooling rate during the cooling process is 2-10°C / min.

Citation Information

Patent Citations

  • Al2O3-Dy2O3-SiO2 ternary system rare-earth sealing material and preparation method of glass sealing ring thereof

    CN101759367A

  • Method for preparing zirconia toughened alumina dental infiltrated ceramic

    CN108726998A

  • Preparation method of alumina / glass composite material and application of alumina / glass composite material in repair of internal cracks of alumina ceramics

    CN115490538A

  • Process for producing a gas and liquid-tight connection between a tube made of ZrO 62° representing an electrolyte and a tube made of Al 62° O 63° surrounding it in an EMF probe M

    DE2114542A1

  • Composition for the protection against corrosion of an article and process for protection thereof

    EP4112692A1

Cited By

  • A method for two-step joining of alumina ceramics based on the principle of alumina powder solder sintering and glass infiltration