Sulfonate grafted organic silicon flame retardant as well as preparation method and application thereof

By grafting sulfonate and a third monomer onto the silicone core to form a core-shell structure of sulfonate-grafted silicone flame retardant, the problem of insufficient flame retardant performance of polycarbonate at low addition amounts is solved. , achieving UL94 V0 level flame retardant effect and improving compatibility and stability with polycarbonate.

CN118755031APending Publication Date: 2024-10-11SHINE POLYMER (ZHUHAI) CO LTD

Patent Information

Application Number
CN202410760262.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, it is difficult for polycarbonate flame retardants to reach the UL94 V0 level at low addition amounts, especially the flame retardant performance for thinner parts is insufficient, and some flame retardants have poor compatibility with polycarbonate. , affecting transparency and appearance.

Method used

By co-grafting the sulfonate and the third monomer onto the silicone core, a sulfonate-grafted silicone flame retardant with a core-shell structure is formed, utilizing the synergistic flame retardant effect of organic silicon and sulfonate. Achieve UL94 V0 level flame retardant performance at low addition amount, and improve compatibility with polycarbonate.

Benefits of technology

The UL94 V0 level flame retardant performance of 1.2mm thin-walled products can be achieved under the condition of adding less than 0.3%, without affecting the physical and mechanical properties of the resin, and improving the uniform dispersion and stability of the flame retardant.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004890847410000051
    Figure BDA0004890847410000051
  • Figure BDA0004890847410000111
    Figure BDA0004890847410000111
  • Figure BDA0004890847410000131
    Figure BDA0004890847410000131
Patent Text Reader

Abstract

The invention discloses a sulfonate grafted organic silicon flame retardant as well as a preparation method and application thereof, and belongs to the technical field of thermoplastic resin products. The sulfonate grafted organic silicon flame retardant disclosed by the invention is of a core-shell structure and comprises organic silicon serving as an inner core, sulfonate serving as a shell and grafted on the surface of the organic silicon and a third monomer, and when the sulfonate grafted organic silicon flame retardant is dispersed in a thermoplastic resin material, the sulfonate grafted organic silicon flame retardant, the sulfonate and the third monomer can play a synergistic flame-retardant role; the flame retardant can realize the UL94V0 flame retardant level of 1.2 mm thin-wall products under the condition of low addition amount, and the physical properties and mechanical properties of matrix resin are not influenced by the addition of the flame retardant.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of thermoplastic resin products, and in particular to a sulfonate grafted organosilicon flame retardant and a preparation method and application thereof, especially application in thermoplastic resin products. Background Art

[0002] Polycarbonate (PC) is a type of thermoplastic engineering plastic with good comprehensive performance, good mechanical properties, excellent heat resistance and electrical resistance, as well as high transparency, high impact strength, low creep and other characteristics. It is widely used in electronic appliances, industrial machinery parts, medical equipment, automobile industry, construction industry and other fields. Polycarbonate itself has a certain self-extinguishing property, but with the improvement of flame retardant requirements, it is still difficult to meet the flame retardant performance requirements in some fields, so it is necessary to modify polycarbonate to make it flame retardant.

[0003] Flame retardants are a type of functional additives that give flammable polymers flame retardancy. According to the application method, they are divided into additive flame retardants and reactive flame retardants. Currently, the additive flame retardants commonly used in polycarbonate are mainly halogen, phosphorus, sulfonate, and silicon. Halogen flame retardants have good flame retardant effects, but they are highly polluting to the environment and are now being phased out. Phosphorus flame retardants are added in large amounts and have low decomposition temperatures. They cause great damage to the mechanical properties and mechanical properties of materials and are prone to corroding molds. Halogen-free and phosphorus-free are the research hotspots of flame retardants in the future. In addition, a series of inorganic and organic sulfonates have also been found to be extremely effective flame retardants for polycarbonate, such as alkali metals or alkaline earth metals of aromatic sulfonic acids, aromatic ketone sulfonic acids, aromatic sulfuric acids, and aromatic ester sulfonic acids, especially alkali metals or alkaline earth metal salts of aromatic sulfone sulfonic acids with electron-withdrawing groups (see US3948851A), which have extremely high flame retardant efficiency. At present, the sulfonate flame retardants commonly used in industry mainly include potassium perfluorobutyl sulfonate (PPFBS), potassium 3-phenylsulfonylbenzene sulfonate (KSS), and sodium 2,4,5-trichlorobenzene sulfonate (STB). In addition, some new sulfonates have also been studied and developed, such as CN102977575A discloses a sulfonate flame retardant containing a triazine ring structure, the synthesis process of the flame retardant is simple, and the sulfonate flame retardant can also form a synergistic flame retardant effect with nitrogen. The sulfonate flame retardant has a small addition amount, high flame retardant efficiency, and little effect on the mechanical properties and light transmittance of polycarbonate. It is suitable for transparent PC flame retardant. The disadvantage is that it cannot reach the UL94 V0 level for thin-walled parts. Some sulfonate flame retardants have poor compatibility with polycarbonate and will exist in the form of crystal points on the surface of polycarbonate parts, affecting the transparency and appearance of polycarbonate; conventional sulfonate flame retardants are also prone to migration in the matrix resin, which leads to a decrease in the flame retardant performance of the parts in the matrix resin. Silicon flame retardants mainly include inorganic silicon flame retardants and organic silicon flame retardants. Inorganic silicon flame retardants mainly include layered silicates (such as montmorillonite), silicon dioxide, silica gel, talc, etc., which can significantly improve the flame retardant properties of resins when added in high amounts, but will also affect the light transmittance and mechanical properties of resins. Organic silicon is mainly polysiloxane, including silicone oil, silicone resin, silicone rubber and a variety of siloxane copolymers, and the fastest growing is organic polysiloxane, such as CN110294846A discloses a cage-shaped silsesquioxane flame retardant, which is non-toxic and halogen-free, has good flame retardant effect, and has good compatibility with polymer matrix, simple preparation method, and is suitable for large-scale production, but when used alone as a flame retardant, it needs to be added to more than 3% to achieve UL94 3.2mm V0 flame retardant level. However, high addition of silicon-based flame retardants (≥0.5%) will lead to a decrease in the mechanical properties of the base resin, and the price of organosiloxane itself is relatively high, resulting in poor economic efficiency of the flame retardant resin.

[0004] Liu Chunlei et al. from Beijing University of Chemical Technology (Liu Chunlei et al., Halogen-free Flame-retardant Polycarbonate Thin-wall Materials, Plastics, Vol. 39, No. 6, 2010) reported that 5-7 parts of silicone resin (methylphenyl silicone resin) can make halogen-free flame-retardant PC thin-wall materials reach UL94 1.6mm V-0 flame retardancy and 0.8mm V-1 flame retardancy. The use of sulfonate (KSS) and silicone resin compounding can show a synergistic effect, so that the addition amount of silicone resin is not more than 1 part, the halogen-free flame-retardant PC thin-wall material can reach UL94 1.6mm V-0 flame retardancy and 0.8mm V-1 flame retardancy. However, the sulfonate and silicone resin compounding system may have poor compatibility with PC thin-wall materials, and the flame retardant mechanisms of sulfonate and silicone resin are different. If the addition ratio of the two is not appropriate, the two flame retardants may antagonize and cause the flame retardant effect to deteriorate. Yang Shanzhi and others from Zhejiang Xin'an Chemical Group Co., Ltd. (Yang Shanzhi et al., Environmentally friendly methylphenyl silicone flame retardant, scientific and technological achievements, 2016-11-19) grafted sulfonate to the silicone resin system through chemical reaction, solving the current problem of compounding silicone (referring to methylphenyl silicone) and sulfonate. It has good compatibility in PC plastics, and the addition amount of 0.3% can reach the UL94 1.6mm V0 flame retardant level. However, this scientific and technological achievement still cannot reach the UL94 V0 flame retardant level of 1.2mm thin-walled products. Summary of the invention

[0005] In view of one or more problems existing in the prior art, the present invention provides a sulfonate grafted silicone flame retardant and a preparation method and application thereof, wherein the sulfonate grafted silicone flame retardant provided uses silicone monomers to polymerize into silicone cores in the presence of crosslinking monomers and / or silane coupling agents during the preparation process, and sulfonates (containing double bonds) and third monomers (containing double bonds) are grafted on the surface of the silicone core as the shell structure of the flame retardant, so that silicone, sulfonates and third monomers can be organically combined into a high molecular polymer flame retardant, and when the flame retardant is dispersed in a thermoplastic resin material, the combination of the three is still tight, which is conducive to the synergistic flame retardant effect during the combustion process, so that the flame retardant can achieve the UL94 V0 flame retardant level of 1.2mm thin-walled products under low addition conditions (e.g., less than 0.3%). The present invention is mainly achieved through the following technical solutions.

[0006] In a first aspect, the present invention provides a sulfonate grafted silicone flame retardant, which is a core-shell structure, comprising silicone as a core and sulfonate and a third monomer grafted on the surface of the silicone as a shell, wherein based on the weight of the sulfonate grafted silicone flame retardant, the content of the silicone is 5-70wt%, optionally 5-40wt%, further optionally 5-35wt%, and further preferably 8-35wt%, the content of the sulfonate is 5-50wt%, optionally 10-50wt%, further optionally 30-50wt%, the content of the third monomer is 10-90wt%, optionally 30-70wt%, further optionally 30-50wt%, and further preferably 30-45wt%; and the third monomer is selected from aromatic vinyl compounds, acrylic acid and its ester compounds and acrylonitrile, and any combination thereof.

[0007] In some embodiments, the organosilicon is obtained by crosslinking an organosilicon monomer in the presence of a crosslinking monomer and / or a silane coupling agent. When the organosilicon monomer used does not contain a double bond, the organosilicon can be obtained by crosslinking an organosilicon monomer in the presence of a crosslinking monomer and a silane coupling agent; when the organosilicon monomer used contains a double bond, the organosilicon can be obtained by crosslinking an organosilicon monomer in the presence of at least one of a crosslinking monomer and a silane coupling agent.

[0008] In some embodiments, the organosilicon monomer is selected from one or more of the following: hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, hexaethylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, dimethyldimethoxysilane, dimethyldiethoxysilane, divinyldimethyloxysilane, divinyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane, decaphenylcyclopentasiloxane, 1,3,5-trimethyl-1,3,5-triphenylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, 8-tetramethyl-2,4,6,8-tetraphenylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetraphenylcyclotetrasiloxane, diphenyldimethoxysilane, diphenyldiethoxysilane, phenylmethyldimethoxysilane, phenylmethyldiethoxysilane, phenylvinyldimethoxysilane and phenylvinyldiethoxysilane; further can be selected from one or more of the following: hexamethylcyclotrisiloxane, a mixture of octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane (i.e., a dimethylcyclosiloxane mixture (DMC)), hexaethylcyclotrisiloxane, methylvinylcyclotetrasiloxane, phenylmethyldimethoxysilane and phenylvinyldimethoxysilane.

[0009] In some embodiments, the crosslinking monomer does not contain a double bond and may be selected from one or more of the following: methyltrimethoxysilane and methyltriethoxysilane.

[0010] In some embodiments, the silane coupling agent contains a double bond and can be selected from one or more of the following: vinyl trimethoxysilane, vinyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane and γ-methacryloxypropyl triisopropoxysilane; and can further be selected from one or more of the following: vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

[0011] In some embodiments, the sulfonate is grafted onto the surface of the organosilicon through copolymerization of its double bonds with double bonds on the surface of the organosilicon, and the third monomer is grafted onto the surface of the organosilicon through ternary copolymerization with the sulfonate and double bonds on the surface of the organosilicon.

[0012] In some embodiments, the sulfonate contains a double bond selected from one or more of the following: vinyl sulfonate, allyl sulfonate, methyl allyl sulfonate, butene disulfonate, R1-CH=CH-(CH2) n -α-olefin sulfonate of the structure shown in FIG. 3M, wherein R1=C9-13 branched or straight chain alkyl, n=1, 2, 3, and M represents an alkali metal or alkaline earth metal, p-styrene sulfonate, and derivatives thereof having substituents on the aromatic group; optionally, the cation in the sulfonate is selected from an alkali metal or an alkaline earth metal; preferably, the alkali metal is selected from: lithium, sodium, and potassium.

[0013] In some embodiments, the aromatic vinyl compound is selected from one or more of the following: styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-ethylstyrene, 4-tert-butylstyrene, 3,4-dimethylstyrene, 4-methoxystyrene, 4-ethoxystyrene, 4-hydroxymethylstyrene, divinylbenzene and 1-vinylnaphthalene.

[0014] In some embodiments, the acrylic acid and its ester compounds are selected from one or more of the following: acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl methacrylate, n-butyl acrylate, isobutyl methacrylate, isobutyl acrylate, isooctyl methacrylate, isooctyl acrylate, dodecyl methacrylate, dodecyl acrylate, hexadecyl methacrylate, hexadecyl acrylate, octadecyl methacrylate, octadecyl acrylate, glycidyl methacrylate, glycidyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl methacrylate and 2-hydroxypropyl acrylate.

[0015] In a second aspect, the present invention provides a method for preparing a sulfonate grafted silicone flame retardant, comprising the following steps:

[0016] S1: mixing an emulsifier, a catalyst and water and heating them to obtain a mixed solution;

[0017] S2: pre-emulsifying the organosilicon monomer, the cross-linking monomer and / or the silane coupling agent, water and the emulsifier to obtain an emulsion, and adding the obtained emulsion to the mixed solution obtained in step S1 to react to obtain an organosilicon emulsion;

[0018] S3: adding the sulfonate, the initiator, the emulsifier and the third monomer into the organic silica gel emulsion obtained in step S2 for grafting reaction to obtain a sulfonate grafted organic silicone emulsion;

[0019] S4: adding the sulfonate grafted silicone emulsion obtained in S3 to an aqueous solution containing a coagulant, heating and stirring to obtain a suspension; and

[0020] S5: centrifuging and drying the suspension obtained in step S4 to obtain the sulfonate grafted silicone flame retardant.

[0021] In some embodiments, in step S1:

[0022] The emulsifier is selected from one or more of anionic surfactants and nonionic surfactants; optionally, the anionic surfactant is selected from sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium benzene sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl diphenyl ether disulfonate, sodium dodecyl polyoxyethylene ether sulfate, sodium fatty alcohol isethionate and disodium dodecyl alcohol polyoxyethylene ether sulfosuccinate; the nonionic surfactant is selected from fatty alcohol polyoxyethylene ether and coconut fatty acid monoethanolamide; further optionally, the amount of the emulsifier in step S1 is 0.01-5 parts by weight, optionally 0.1-1.0 parts by weight, relative to 100 parts by weight of the sum of the organosilicon monomer, crosslinking monomer and / or silane coupling agent; and / or

[0023] The heating temperature is 30-95°C, and can be 50-90°C; and / or

[0024] The catalyst is selected from one or more of the following: tetramethylammonium hydroxide, tetraethylammonium hydroxide, lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, dodecyl sulfonic acid, dodecylbenzene sulfonic acid, sulfuric acid, hydrochloric acid, or any combination thereof; optionally, the amount of the catalyst is 0.02-5 parts by weight, optionally 0.5-1.5 parts by weight, relative to 100 parts by weight of the sum of the organosilicon monomer, crosslinking monomer and / or silane coupling agent.

[0025] In some embodiments, in step S2:

[0026] The amount of the emulsifier is 0.1-0.5 parts by weight relative to 100 parts by weight of the total amount of the silicone monomer, the crosslinking monomer and / or the silane coupling agent; and / or

[0027] The total amount of the crosslinking monomer and / or the silane coupling agent is 10-30 parts by weight relative to 100 parts by weight of the organic silicon monomer; and / or

[0028] The reaction conditions are: reacting at 50-90°C; and / or

[0029] The concentration of organic silicon in the organic silicon latex is 15-45%.

[0030] In some embodiments, in step S3:

[0031] The initiator is selected from one or more of the following: hydrogen peroxide, potassium persulfate, ammonium persulfate, azobisisobutyronitrile, cumene hydroperoxide, tert-butyl hydroperoxide and benzoyl peroxide; optionally, the amount of the initiator is 0.05-3.0 parts by weight, optionally 0.1-1.0 parts by weight, relative to 100 parts by weight of the total amount of the sulfonate and the third monomer; and / or

[0032] The amount of the emulsifier is 0.05-3.0 parts by weight, and can be 0.2-0.5 parts by weight, relative to 100 parts by weight of the total amount of the sulfonate and the third monomer; and / or

[0033] Relative to 100 parts by weight of the total amount of the organosilicon monomer, the sulfonate and the third monomer, the amount of the organosilicon monomer is 5-70 parts by weight, optionally 5-40 parts by weight, further optionally 5-35 parts by weight, further preferably 8-35 parts by weight, further more preferably 10-30 parts by weight, for example 14-26 parts by weight, the amount of the sulfonate is 5-50 parts by weight, optionally 10-50 parts by weight, further optionally 30-50 parts by weight, for example 33-48 parts by weight, the amount of the third monomer is 10-90 parts by weight, optionally 30-70 parts by weight, further optionally 30-50 parts by weight, further preferably 30-45 parts by weight, for example 31-43 parts by weight; and / or

[0034] The grafting reaction is carried out under the conditions of 50-90° C. for 2-4 hours.

[0035] In some embodiments, in step S4;

[0036] The coagulant is selected from one or more of the following: sodium chloride, magnesium chloride, calcium chloride, ferric chloride, ferrous chloride, aluminum chloride, cupric chloride, magnesium sulfate, aluminum sulfate, calcium acetate, cupric sulfate, ferric sulfate, ferrous sulfate, sodium phosphate, calcium phosphate and magnesium phosphate; optionally, the concentration of the coagulant in the aqueous solution containing the coagulant is 0.2-8%, and can further be 2-8%.

[0037] In a third aspect, the present invention provides a thermoplastic resin composition comprising the following raw materials in parts by weight:

[0038]

[0039] The flame retardant is the sulfonate grafted silicone flame retardant provided by the first aspect of the present invention or the sulfonate grafted silicone flame retardant prepared by the method provided by the second aspect of the present invention.

[0040] In some embodiments, the thermoplastic resin includes polycarbonate resin (PC), acrylonitrile-butadiene-styrene copolymer resin (ABS), PC / ABS alloy, rubber-modified polystyrene resin, acrylonitrile-styrene-acrylate copolymer resin, methyl methacrylate-butadiene-styrene copolymer resin, acrylonitrile-ethyl acrylate-styrene copolymer resin, copolymers thereof, or combinations thereof.

[0041] In a fourth aspect, the present invention provides a thermoplastic resin article produced from the thermoplastic resin composition provided in the third aspect of the present invention. DETAILED DESCRIPTION

[0042] The concentrated aqueous dispersion of fluorine-containing polymers provided by the present invention and its preparation method and application are described below by specific embodiments. However, the following description is provided for those skilled in the art to fully understand the present application and is not intended to limit the subject matter described in the claims.

[0043] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0044] In this specification, unless otherwise specified, "%" means "mass % (also expressed as wt %)".

[0045] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0047] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0048] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0049] In the description of this article, it should be noted that, unless otherwise specified, "above" and "below" are inclusive of the number, and "several" in "one or several" means two or more.

[0050] Among the additive flame retardants currently commonly used in polycarbonate, halogen flame retardants are gradually being eliminated due to their serious environmental pollution; phosphorus flame retardants have a large addition amount and a low decomposition temperature, which will cause great damage to the mechanical properties and mechanical properties of the material and easily corrode the mold; although sulfonate flame retardants have a high flame retardant efficiency, they cannot reach the UL94 V0 level for thin-walled parts (such as 1.2mm thin-walled parts), and some sulfonate flame retardants have poor compatibility with materials such as polycarbonate, and will exist in the form of crystal points on the surface of polycarbonate parts, affecting the transparency and appearance of polycarbonate; silicon flame retardants can also achieve a high flame retardant effect, but when used alone, they need to be added to more than 3% to achieve the UL94 3.0mm V0 flame retardant level, and high addition amounts will lead to a decrease in the mechanical properties of the base resin; although the flame retardant properties of the silicone resin system can be improved by chemically grafting sulfonates to the silicone resin system, an addition amount of 0.3% can reach UL94 1.6mm V0 flame retardant grade, however, it is still difficult to achieve UL94 V0 level for thinner parts (such as 1.2mm thin-walled parts).

[0051] The inventors have noticed through extensive research that the sulfonate-grafted silicone flame retardant obtained by grafting a sulfonate containing double bonds and a third monomer onto the surface of an organosilicon core (obtained by crosslinking an organosilicon monomer or a combination of multiple thereof in the presence of a crosslinking monomer and / or a silane coupling agent) through a chemical reaction (wherein the double bonds of the sulfonate, the double bonds of the third monomer and the double bonds on the surface of the organosilicon core are ternary copolymerized) can achieve a UL94 rating for products of 1.6 mm or thinner (e.g., 1.2 mm) at a low addition amount. V0 flame retardant grade, in which the silicone core as a silicon-based flame retardant element and the grafted sulfonate as a sulfonate flame retardant element produce a silicon-sulfonate synergistic flame retardant effect during combustion, achieving more efficient flame retardancy, and the copolymerized third monomer can increase the compatibility of the flame retardant with the matrix resin, so that the flame retardant is more evenly dispersed in the matrix resin, thereby further improving the flame retardant effect and achieving a stable flame retardant effect, and the sulfonate grafted silicone flame retardant is not easy to migrate in thermoplastic resin products, and does not affect the physical and mechanical properties of the resin products.

[0052] Example

[0053] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.

[0054] Example 1: Preparation of sulfonate grafted silicone flame retardant

[0055] (1) Preparation of 20 wt% (solid content of organic silica gel emulsion, the same below) organic silica gel emulsion

[0056] 1.1) In a 2L three-necked flask equipped with a stirrer and a thermometer, add 500g of deionized water, 0.3g of sodium dodecyl sulfate and 1.2g of sulfuric acid, start stirring and heat to 60°C.

[0057] 1.2) 200g of deionized water, 170g of DMC (dimethylcyclosiloxane mixture, also known as dimethylsiloxane mixed ring body, a mixture of hexamethylcyclotrisiloxane (D3), octamethylcyclotetrasiloxane (D4) and decamethylcyclopentasiloxane (D5), purchased from Tangshan Sanyou Chemical Co., Ltd.), 5g of methyltrimethoxysilane (Shanghai Aladdin Reagent Co., Ltd.), 30g of vinyltrimethoxysilane (Shanghai Aladdin Reagent Co., Ltd.), and 0.4g of sodium dodecyl sulfate were uniformly added dropwise to a three-necked flask containing the mixed solution obtained in step 1.1) within 2 hours. After the addition was completed, the temperature was raised to 70°C and kept warm for 2 hours to obtain an organic silica gel emulsion, in which the concentration of organic silicon was about 20wt%.

[0058] (2) Preparation of flame retardants

[0059] 2.1) All of the 20 wt% organic silica gel emulsion prepared in (1) above, 2.0 g sodium lauryl sulfate, 500 g deionized water and 2 g potassium persulfate were added to a 5 L three-necked flask with a stirrer and a thermometer and the temperature was raised to 65°C.

[0060] 2.2) 500 g of a 20% aqueous solution of sodium p-styrene sulfonate (Shanghai Aladdin Reagent Co., Ltd.) and 500 g of styrene were uniformly added dropwise to the three-necked flask containing the mixed solution obtained in step 2.1). After about three hours of addition, the temperature was raised to 75° C. and kept warm for 2 hours to obtain a sulfonate-grafted silicone emulsion.

[0061] 2.3) The sulfonate grafted silicone emulsion obtained in 2.2) was poured into 1L 3% calcium chloride aqueous solution at 70°C, stirred for half an hour to obtain a suspension, and the suspension was centrifuged in a centrifuge at a speed of not less than 600rpm, and the centrifugal precipitate was collected, and the mother liquor was clarified, indicating that the sulfonate monomer (sodium p-styrene sulfonate) and the third monomer (styrene) used were basically grafted to the surface of the silicone core through their double bond copolymerization, and then the precipitate was dried in a drying oven at 70-120°C to obtain a sulfonate grafted silicone flame retardant, named flame retardant A. The content ratio of the silicone core, the sulfonate grafted on the surface of the silicone core, and the third monomer in the obtained flame retardant can be quantitatively determined by infrared spectroscopy. The results show that the ratio of the silicone core, the grafted sulfonate and the third monomer in the obtained flame retardant is basically consistent with the weight ratio of the raw materials used, so the content ratio of the silicone core, the grafted sulfonate and the third monomer in the prepared flame retardant can be determined by the amount of the silicone monomer, the sulfonate monomer and the third monomer used in the preparation of the flame retardant.

[0062] Example 2: Preparation of sulfonate grafted silicone flame retardant

[0063] (1) Preparation of 40 wt% (solid content of organic silica gel emulsion, the same below) organic silica gel emulsion

[0064] 1.1) In a 2L three-necked flask equipped with a stirrer and a thermometer, add 500g of deionized water, 0.6g of sodium dodecyl sulfate and 3.0g of sulfuric acid, start stirring and raise the temperature to 60°C.

[0065] 1.2) A pre-emulsion prepared by mixing 200 g of deionized water, 340 g of DMC, 30 g of methyltrimethoxysilane, 60 g of vinyltrimethoxysilane and 0.6 g of sodium dodecyl sulfate was uniformly added dropwise to a three-necked flask containing the mixed solution obtained in step (1.1) within 2 hours. After the addition was completed, the temperature was raised to 70° C. and kept warm for 2 hours to obtain an organic silica gel emulsion in which the concentration of organic silicone was about 40 wt %.

[0066] (2) Preparation of flame retardants

[0067] 2.1) All 40 wt% of the organic silica gel emulsion prepared in (1) above, 3.6 g of sodium lauryl sulfate, 500 g of deionized water and 5 g of potassium persulfate were added to a 5 L three-necked flask with a stirrer and a thermometer and the temperature was raised to 65°C.

[0068] 2.2) 600 g of a 20% aqueous solution of sodium p-styrene sulfonate and 500 g of styrene were added dropwise to the mixed solution obtained in step (2.1) in a three-necked flask. After about three hours of addition, the temperature was raised to 75° C. and kept at this temperature for 2 hours to obtain a sulfonate-grafted silicone emulsion.

[0069] 2.3) The sulfonate grafted silicone emulsion obtained in 2.2) was poured into 1L 5% calcium chloride aqueous solution at 70°C, stirred for half an hour to obtain a suspension, and the suspension was centrifuged in a centrifuge at a speed of not less than 600rpm, and the centrifugal precipitate was collected and the mother liquor was clarified, indicating that the sulfonate monomer (sodium p-styrene sulfonate) and the third monomer (styrene) used were basically grafted to the surface of the silicone core through their double bond copolymerization, and then the precipitate was dried in a drying oven at 70-120°C to obtain a sulfonate grafted silicone flame retardant, named flame retardant B. The content ratio of the silicone core, the sulfonate grafted on the surface of the silicone core and the third monomer in the obtained flame retardant can be quantitatively determined by infrared spectroscopy, and the results show that the ratio of the silicone core, the grafted sulfonate and the third monomer in the obtained flame retardant is also basically consistent with the weight ratio of the raw materials used.

[0070] Example 3

[0071] The preparation process of Example 3 is substantially the same as that of Example 1, except that:

[0072] In step 1.2), hexaethylcyclotrisiloxane (Shanghai Aladdin Reagent Co., Ltd.) was used instead of DMC in Example 1, and the amount of vinyltrimethoxysilane used was 15 g;

[0073] The flame retardant obtained in this example is named flame retardant C.

[0074] Example 4

[0075] The preparation process of Example 4 is substantially the same as that of Example 1, except that:

[0076] In step 1.2), methylvinylcyclotetrasiloxane (Shanghai Aladdin Reagent Co., Ltd.) was used instead of DMC in Example 1, and methyltrimethoxysilane was not used;

[0077] The flame retardant obtained in this example is named flame retardant D.

[0078] Example 5

[0079] The preparation process of Example 5 is substantially the same as that of Example 1, except that:

[0080] The amount of sodium lauryl sulfate used in step 1.1) is 1.97 g, and the amount of sulfuric acid used is 2.8 g;

[0081] In step 1.2), the amount of sodium dodecyl sulfate used is 0.92 g, the amount of vinyltrimethoxysilane used is 20 g, and the amount of methyltrimethoxysilane used is 7 g;

[0082] The amount of potassium persulfate used in step 2.1) is 1.0 g, and the amount of sodium dodecyl sulfate used is 5 g;

[0083] In step 2.2), 550 g of a 20% aqueous solution of sodium p-styrene sulfonate and 450 g of styrene are added dropwise to the three-necked flask containing the mixed solution obtained in step 2.1);

[0084] The concentration of the calcium chloride aqueous solution used in step 2.3) is 8%;

[0085] The flame retardant obtained in this example is named flame retardant E.

[0086] Example 6

[0087] The preparation process of Example 6 is substantially the same as that of Example 2, except that:

[0088] In step 1.2), the amount of vinyltrimethoxysilane used is 60 g, and the amount of methyltrimethoxysilane used is 30 g;

[0089] In step 2.2), 750 g of a 20% aqueous solution of sodium p-styrene sulfonate and 510 g of styrene are added dropwise to the three-necked flask containing the mixed solution obtained in step 2.1);

[0090] The flame retardant obtained in this example is named flame retardant F.

[0091] Example 7

[0092] The preparation process of Example 7 is substantially the same as that of Example 2, except that:

[0093] In step 2.2), 450 g of a 20% aqueous solution of sodium p-styrene sulfonate and 540 g of styrene are added dropwise to the three-necked flask containing the mixed solution obtained in step 2.1);

[0094] The concentration of the calcium chloride aqueous solution used in step 2.3) is 2%;

[0095] The flame retardant obtained in this example is named flame retardant G.

[0096] Example 8

[0097] The preparation process of Example 8 is basically the same as that of Example 1, except that γ-methacryloxypropyltrimethoxysilane (Shanghai Aladdin Reagent Co., Ltd.) is used instead of vinyltrimethoxysilane in Example 1, and the obtained flame retardant is named flame retardant H.

[0098] Example 9

[0099] The preparation process of Example 9 is basically the same as that of Example 1, except that methyltriethoxysilane (Shanghai Aladdin Reagent Co., Ltd.) is used instead of the methyltrimethoxysilane in Example 1, and the obtained flame retardant is named Flame Retardant I.

[0100] Example 10

[0101] The preparation process of Example 10 is basically the same as that of Example 1, except that sodium allyl sulfonate (Shanghai Aladdin Reagent Co., Ltd.) is used instead of sodium p-styrene sulfonate in Example 1, and the obtained flame retardant is named flame retardant J.

[0102] Embodiment 11

[0103] The preparation process of Example 11 is basically the same as that of Example 1, except that methyl methacrylate (Shanghai Aladdin Reagent Co., Ltd.) is used instead of styrene in Example 1, and the obtained flame retardant is named flame retardant K.

[0104] Example 12

[0105] The preparation process of Example 12 is basically the same as that of Example 1, except that phenylvinyldimethoxysilane (Shanghai Aladdin Reagent Co., Ltd.) is used instead of DMC in Example 1, and methyltrimethoxysilane is not used in step 1.2). The obtained flame retardant is named flame retardant L.

[0106] Embodiment 13

[0107] The preparation process of Example 13 is basically the same as that of Example 1, except that phenylmethyldimethoxysilane (Shanghai Aladdin Reagent Co., Ltd.) is used instead of DMC in Example 1, and the obtained flame retardant is named flame retardant M.

[0108] Embodiment 14

[0109] The preparation process of Example 14 is basically the same as that of Example 1, except that acrylonitrile (Shanghai Aladdin Reagent Co., Ltd.) is used instead of styrene in Example 1, and the obtained flame retardant is named Flame Retardant N.

[0110] Comparative Example 1

[0111] Comparative Example 1 is a commercially available potassium 3-phenylsulfonylbenzenesulfonate (KSS) flame retardant (Shanghai MacLean Biochemical Technology Co., Ltd.).

[0112] Comparative Example 2

[0113] Comparative Example 2 is a commercially available potassium perfluorobutanesulfonate (KPFBS) flame retardant (Shanghai MacLean Biochemical Technology Co., Ltd.).

[0114] Comparative Example 3

[0115] Comparative Example 3 is a commercially available polymethylphenylsilane (PPMS) flame retardant (Shanghai Aladdin Reagent Co., Ltd.).

[0116] Comparative Example 4

[0117] The preparation process of Comparative Example 4 is substantially the same as that of Example 1, except that the third monomer styrene is not used in the preparation of the flame retardant.

[0118] Comparative Example 5

[0119] The preparation process of Comparative Example 5 is substantially the same as that of Example 12, except that the third monomer styrene is not used in the preparation of the flame retardant.

[0120] Comparative Example 6

[0121] The preparation process of Comparative Example 6 is substantially the same as that of Example 13, except that potassium 3-phenylsulfonylbenzenesulfonate (containing no double bond) is used instead of sodium p-styrenesulfonate in step 2.2).

[0122] Comparative Example 7

[0123] The preparation process of Comparative Example 7 is basically the same as that of Example 13, except that potassium 3-phenylsulfonylbenzenesulfonate (containing no double bond) is used instead of sodium p-styrenesulfonate in step 2.2), and the third monomer styrene is not used in the preparation of the flame retardant.

[0124] Example 15: Preparation of thermoplastic resin products containing flame retardants

[0125] The flame retardant-containing thermoplastic resin product provided in this embodiment is made of a thermoplastic resin composition comprising the following raw materials in parts by weight:

[0126]

[0127] The thermoplastic resin composition composed of the above raw materials in parts by weight was extruded and granulated at 270°C using a Nanjing Jieente SHJ-36 plastic extruder, and injection molded at 280°C using a Haitian SA860 injection molding machine to obtain a thermoplastic resin product containing a flame retardant. The physical and chemical properties (including fluidity, flame retardancy, mechanical properties, etc.) of the thermoplastic resin product were tested, and the results are shown in Table 1 below.

[0128] Test methods for physical and chemical properties of thermoplastic resin products:

[0129] (1.1) Flame retardant performance (vertical burning 1.6mm, vertical burning 1.2mm)

[0130] Test standard: UL 94-2020;

[0131] Test equipment: RH-6033B horizontal combustion tester;

[0132] Test conditions:

[0133] Pretreatment: Place the test sample in an environment of 23±2℃, 50±10% RH for 48h; age it at 70℃ for 168h, and then place it in a desiccator for at least 4h to cool to room temperature;

[0134] Test steps: Place a Bunsen burner (flame height 20±1mm) at the exact center below the sample, with the mouth of the Bunsen burner 10±1mm away from the bottom of the sample. The ignition time is 10±0.5s. After 10±0.5s of ignition, move the Bunsen burner at least 150mm away at a speed of 300mm / sec. At the same time, start recording the afterflame time t1. When the afterflame stops, ignite it immediately for 10±0.5s. After 10±0.5s of ignition, move the Bunsen burner at least 150mm away at a speed of 300mm / sec. At the same time, record the afterflame time t2 and afterburning time t3. Calculate the flame retardant properties of the test sample according to the UL94-2020 test standard.

[0135] (1.2) Izod notched impact strength

[0136] Test standard: ASTM D256-10(2018);

[0137] Testing equipment: Zwick HIT 25P plastic pendulum impact tester;

[0138] (1.3) Melt mass flow rate

[0139] Test standard: ASTM D1238-13;

[0140] Testing equipment: MFLOW melt flow rate tester / FD-115 drying oven;

[0141] (1.4) Vicat softening temperature

[0142] Test standard: ASTM D1525-17;

[0143] Testing equipment: 40-197-100 thermal deformation Vicat testing machine;

[0144] Examples 16-28

[0145] Examples 16-28 are carried out according to the method steps of Example 15, except that different flame retardants are used in preparing the thermoplastic resin product, specifically: Example 16 uses flame retardant B, Example 17 uses flame retardant C, Example 18 uses flame retardant D, Example 19 uses flame retardant E, Example 20 uses flame retardant F, Example 21 uses flame retardant G, Example 22 uses flame retardant H, Example 23 uses flame retardant I, Example 24 uses flame retardant J, Example 25 uses flame retardant K, Example 26 uses flame retardant L, Example 27 uses flame retardant M, and Example 28 uses flame retardant N. The test results of the physical and chemical properties of the thermoplastic resin product are shown in Table 1 below.

[0146] Comparative Examples 8-15

[0147] Comparative Examples 8-15 were carried out according to the method steps of Example 15, except that different types or addition amounts of flame retardants were used in preparing the thermoplastic resin products, specifically:

[0148] Comparative Example 8 used 0.6 parts of KSS.

[0149] Comparative Example 9 used 0.3 parts of KPFBS.

[0150] Comparative Example 10 used 2 parts of PPMS.

[0151] Comparative Example 11 used 0.3 parts of KSS + 0.5 parts of PPMS.

[0152] Comparative Example 12 used 0.3 parts of the flame retardant prepared according to Comparative Example 4.

[0153] Comparative Example 13 used 0.3 parts of the flame retardant prepared according to Comparative Example 5.

[0154] Comparative Example 14 used 0.3 parts of the flame retardant prepared according to Comparative Example 6.

[0155] Comparative Example 15 used 0.3 parts of the flame retardant prepared according to Comparative Example 7.

[0156] Table 1: Test results of physical and chemical properties of thermoplastic resin products prepared in Examples 15-28 and Comparative Examples 8-15

[0157]

[0158] From the test results of the physical and chemical properties of the thermoplastic resin products recorded in Table 1 above, it can be seen that the thermoplastic resin products prepared in Examples 15-28 have no difference in Vicat softening temperature with the thermoplastic resin products prepared in Comparative Examples 8-15. However, the thin-wall flame retardant performance of Examples 15-28 is more excellent, especially the 1.2mm flame retardant performance, which can reach the UL94 1.2mm V0 flame retardant level under the condition of about 0.3% addition. Compared with the existing sulfonate flame retardants, organosilicon flame retardants or their physical combination with sulfonate flame retardants, phenylsilicon copolymer sulfonate flame retardants and sulfonate grafted organosilicon flame retardants (not containing a third monomer grafting, Comparative Examples 12-13) in Comparative Examples 8-15, the flame retardant properties are better. Comparative Examples 8-15 can only achieve UL94 1.2mm V1 flame retardant level at most under the same addition amount or even higher addition amount. In addition, in Comparative Examples 14 and 15, since the 3-phenylsulfonylbenzenesulfonate potassium used does not contain a double bond, it may not be grafted onto the organosilicon core through double bond copolymerization like other sulfonates containing double bonds, resulting in poor flame retardant properties of the prepared flame retardant. These results show that the organic combination of organosilicon, sulfonate containing double bonds and the third monomer in the sulfonate grafted organosilicon flame retardant provided by the present invention can play a synergistic flame retardant role, so that the flame retardant can achieve UL94 of 1.2mm thin-walled products under low addition amount (e.g., 0.3%). V0 flame retardant grade. In addition, it can be seen from Comparative Example 10 that a higher amount of organic silicon flame retardant added reduces the impact performance of the base resin and increases the resin melt index, while the flame retardants in Examples 15-28 do not affect the impact performance (Izod notched impact strength) and melt index (melt mass flow rate) of the base resin. Therefore, compared with existing flame retardants, the sulfonate grafted organic silicon flame retardant provided by the present invention can produce thermoplastic resin products with better comprehensive performance.

[0159] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A sulfonate grafted silicone flame retardant, characterized in that: The sulfonate grafted silicone flame retardant is a core-shell structure, which comprises silicone as a core and sulfonate and a third monomer grafted on the surface of the silicone as a shell, wherein based on the weight of the sulfonate grafted silicone flame retardant, the content of the silicone is 5-70wt%, optionally 5-40wt%, further optionally 5-35wt%, the content of the sulfonate is 5-50wt%, optionally 10-50wt%, further optionally 30-50wt%, and the content of the third monomer is 10-90wt%, optionally 30-70wt%, further optionally 30-50wt%; and The third monomer is selected from aromatic vinyl compounds, acrylic acid and its ester compounds, acrylonitrile, and any combination thereof.

2. The sulfonate grafted silicone flame retardant according to claim 1, characterized in that: The organosilicon is obtained by cross-linking an organosilicon monomer in the presence of a cross-linking monomer and / or a silane coupling agent; Optionally, the organosilicon monomer is selected from one or more of the following: hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, hexaethylcyclotrisiloxane, 2,4,6,8-tetramethyl-2,4,6,8-tetravinylcyclotetrasiloxane, dimethyldimethoxysilane, dimethyldiethoxysilane, divinyldimethyloxysilane, divinyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, hexaphenylcyclotrisiloxane, octaphenylcyclotetrasiloxane, decaphenylcyclopentasiloxane, 1,3,5-trimethyl-1,3,5-triphenylcyclotrisiloxane , 2,4,6,8-tetramethyl-2,4,6,8-tetraphenylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetraphenylcyclotetrasiloxane, diphenyldimethoxysilane, diphenyldiethoxysilane, phenylmethyldimethoxysilane, phenylmethyldiethoxysilane, phenylvinyldimethoxysilane and phenylvinyldiethoxysilane; further can be selected from one or more of the following: a mixture of hexamethylcyclotrisiloxane with octamethylcyclotetrasiloxane and decamethylcyclopentasiloxane, hexaethylcyclotrisiloxane, methylvinylcyclotetrasiloxane, phenylmethyldimethoxysilane and phenylvinyldimethoxysilane; Optionally, the crosslinking monomer is selected from one or more of the following: methyltrimethoxysilane and methyltriethoxysilane; Optionally, the silane coupling agent is selected from one or more of the following: vinyl trimethoxysilane, vinyl triethoxysilane, γ-methacryloxypropyl trimethoxysilane and γ-methacryloxypropyl triisopropoxysilane; and further selected from one or more of the following: vinyl trimethoxysilane and γ-methacryloxypropyl trimethoxysilane.

3. The sulfonate grafted silicone flame retardant according to claim 1 or 2, characterized in that: The sulfonate is grafted onto the surface of the organosilicon through copolymerization of its double bonds with double bonds on the surface of the organosilicon, and the third monomer is grafted onto the surface of the organosilicon through ternary copolymerization of the sulfonate and double bonds on the surface of the organosilicon.

4. The sulfonate grafted silicone flame retardant according to any one of claims 1 to 3, characterized in that: The sulfonate contains a double bond and is selected from one or more of the following: vinyl sulfonate, allyl sulfonate, methyl allyl sulfonate, butene disulfonate, R1-CH=CH-(CH2) n - α-olefin sulfonate with the structure shown in -SO3M, wherein R1 = C9-13 branched or straight chain alkyl, n = 1, 2, 3, M represents an alkali metal or alkaline earth metal, p-styrene sulfonate and its derivatives with substituents on the aromatic group; Optionally, the cation in the sulfonate is selected from alkali metals or alkaline earth metals; preferably, the alkali metal is selected from: lithium, sodium, potassium.

5. The sulfonate grafted silicone flame retardant according to any one of claims 1 to 4, characterized in that: The aromatic vinyl compound is selected from one or more of the following: styrene, α-methylstyrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, 4-ethylstyrene, 4-tert-butylstyrene, 3,4-dimethylstyrene, 4-methoxystyrene, 4-ethoxystyrene, 4-hydroxymethylstyrene, divinylbenzene and 1-vinylnaphthalene; and / or The acrylic acid and its ester compounds are selected from one or more of the following: acrylic acid, methacrylic acid, methyl methacrylate, methyl acrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, n-butyl methacrylate, n-butyl acrylate, isobutyl methacrylate, isobutyl acrylate, isooctyl methacrylate, isooctyl acrylate, dodecyl methacrylate, dodecyl acrylate, hexadecyl methacrylate, hexadecyl acrylate, octadecyl methacrylate, octadecyl acrylate, glycidyl methacrylate, glycidyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl methacrylate and 2-hydroxypropyl acrylate.

6. The method for preparing the sulfonate grafted silicone flame retardant according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1: mixing an emulsifier, a catalyst and water and heating them to obtain a mixed solution; S2: pre-emulsifying the organosilicon monomer, the cross-linking monomer and / or the silane coupling agent, water and the emulsifier to obtain an emulsion, and adding the obtained emulsion to the mixed solution obtained in step S1 to react to obtain an organosilicon emulsion; S3: adding the sulfonate, the initiator, the emulsifier and the third monomer into the organic silica gel emulsion obtained in step S2 for grafting reaction to obtain a sulfonate grafted organic silicone emulsion; S4: adding the sulfonate grafted silicone emulsion obtained in S3 to an aqueous solution containing a coagulant, heating and stirring to obtain a suspension; and S5: centrifuging and drying the suspension obtained in step S4 to obtain the sulfonate grafted silicone flame retardant.

7. The preparation method according to claim 6, characterized in that: In step S1: The emulsifier is selected from one or more of anionic surfactants and nonionic surfactants; optionally, the anionic surfactant is selected from sodium dodecyl sulfonate, sodium dodecyl sulfate, sodium benzene sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl diphenyl ether disulfonate, sodium dodecyl polyoxyethylene ether sulfate, sodium fatty alcohol isethionate and disodium dodecyl alcohol polyoxyethylene ether sulfosuccinate; the nonionic surfactant is selected from fatty alcohol polyoxyethylene ether and coconut fatty acid monoethanolamide; further optionally, the amount of the emulsifier in step S1 is 0.01-5 parts by weight, optionally 0.1-1.0 parts by weight, relative to 100 parts by weight of the sum of the organosilicon monomer, crosslinking monomer and / or silane coupling agent; and / or The heating temperature is 30-95°C, and can be 50-90°C; and / or The catalyst is selected from one or more of the following: tetramethylammonium hydroxide, tetraethylammonium hydroxide, lithium hydroxide, sodium hydroxide, potassium hydroxide, cesium hydroxide, dodecyl sulfonic acid, dodecylbenzene sulfonic acid, sulfuric acid, hydrochloric acid, or any combination thereof; optionally, the amount of the catalyst is 0.02-5 parts by weight, optionally 0.5-1.5 parts by weight, relative to 100 parts by weight of the sum of the organosilicon monomer, crosslinking monomer and / or silane coupling agent.

8. The preparation method according to claim 6 or 7, characterized in that: In step S2: The amount of the emulsifier is 0.1-0.5 parts by weight relative to 100 parts by weight of the total amount of the silicone monomer, the crosslinking monomer and / or the silane coupling agent; and / or The total amount of the crosslinking monomer and / or the silane coupling agent is 10-30 parts by weight relative to 100 parts by weight of the organic silicon monomer; and / or The reaction conditions are: reacting at 50-90°C; and / or The concentration of organic silicon in the organic silicon latex is 15-45%.

9. The preparation method according to any one of claims 6 to 8, characterized in that: In step S3: The initiator is selected from one or more of the following: hydrogen peroxide, potassium persulfate, ammonium persulfate, azobisisobutyronitrile, cumene hydroperoxide, tert-butyl hydroperoxide and benzoyl peroxide; optionally, the amount of the initiator is 0.05-3.0 parts by weight, optionally 0.1-1.0 parts by weight, relative to 100 parts by weight of the total amount of the sulfonate and the third monomer; and / or The amount of the emulsifier is 0.05-3.0 parts by weight, and can be 0.2-0.5 parts by weight, relative to 100 parts by weight of the total amount of the sulfonate and the third monomer; and / or Relative to 100 parts by weight of the total amount of the organosilicon monomer, the sulfonate and the third monomer, the amount of the organosilicon monomer is 5-70 parts by weight, optionally 5-40 parts by weight, further optionally 5-35 parts by weight, the amount of the sulfonate is 5-50 parts by weight, optionally 10-50 parts by weight, further optionally 30-50 parts by weight, and the amount of the third monomer is 10-90 parts by weight, optionally 30-70 parts by weight, further optionally 30-50 parts by weight; and / or The grafting reaction is carried out under the conditions of 50-90° C. for 2-4 hours.

10. The preparation method according to any one of claims 6 to 9, characterized in that: In step S4; The coagulant is selected from one or more of the following: sodium chloride, magnesium chloride, calcium chloride, ferric chloride, ferrous chloride, aluminum chloride, cupric chloride, magnesium sulfate, aluminum sulfate, calcium acetate, cupric sulfate, ferric sulfate, ferrous sulfate, sodium phosphate, calcium phosphate and magnesium phosphate; optionally, the concentration of the coagulant in the aqueous solution containing the coagulant is 0.2-8%, and can further be 2-8%.

11. A thermoplastic resin composition, characterized in that The thermoplastic resin composition comprises the following raw materials in parts by weight: The flame retardant is the sulfonate grafted silicone flame retardant according to any one of claims 1 to 5 or the sulfonate grafted silicone flame retardant prepared by the method according to any one of claims 6 to 10.

12. The thermoplastic resin composition according to claim 11, characterized in that The thermoplastic resin includes polycarbonate resin (PC), acrylonitrile-butadiene-styrene copolymer resin (ABS), PC / ABS alloy, rubber-modified polystyrene resin, acrylonitrile-styrene-acrylate copolymer resin, methyl methacrylate-butadiene-styrene copolymer resin, acrylonitrile-ethyl acrylate-styrene copolymer resin, copolymers thereof, or combinations thereof.

13. A thermoplastic resin article produced from the thermoplastic resin composition according to claim 11 or 12.

Citation Information

Patent Citations

  • Sulfonate fire retardation agents and preparation methods thereof

    CN102977575A

  • Polyhedral oligomeric silsesquioxane-mixed flame retardant containing DOPO (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide) groups and preparation method and application thereof

    CN110294846A

  • Flame retardant polycarbonate composition

    US3948851A

Cited By

  • Organosilicon sulfonate with low-temperature toughening and flame-retardant functions as well as preparation method and application thereof

    CN120192477A

  • Macromolecular flame retardant for transparent antistatic flame-retardant polycarbonate resin and preparation method thereof

    CN121930477A

  • Macromolecular flame retardant for transparent antistatic flame-retardant polycarbonate resin and method for preparing the same

    CN121930477B