Method for removing bimetallic catalyst

The combination of hydrogen peroxide and manganese dioxide removes DMC catalyst residues in polyethers, which solves the environmental and health risks caused by catalyst residues, improves product purity and color, and achieves green and sustainable development of polyether polyol production.

CN118755076APending Publication Date: 2024-10-11NINGBO YUANLI CHEM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411054345.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing technology, the double metal cyanide complex catalyst remains in the polyether, causing environmental and health risks, and decomposes when air oxidizes to produce harmful substances, affecting product performance and appearance.

Method used

Using a combination method of hydrogen peroxide and manganese dioxide, the DMC catalyst residue is removed through stirring and filtration steps, and filter aids are used to remove moisture and improve the purity and color of polyether polyol.

Benefits of technology

It effectively removes catalyst residues, improves product purity and color, eliminates the impact of peroxide, has significant environmental and economic benefits, and promotes the green and sustainable development of polyether polyol production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for removing a bimetallic catalyst, which comprises the following steps of: (1) mixing polyether polyol containing a DMC (Dimethyl Carbonate) catalyst with a hydrogen peroxide solution, and stirring to form floccule; (2) mixing the polyether polyol with manganese dioxide and water for a period of time, and removing peroxide; and (3) adding a filter aid, removing water, and filtering insoluble substances to obtain pure polyether polyol without the DMC catalyst. According to the method, raw materials are easy to obtain, operation is easy and convenient, DMC catalyst residues in polyether polyol can be effectively removed, the product purity and color can be improved, meanwhile, influences of peroxides can be eliminated, and remarkable environmental and economic benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyether polyol synthesis, and in particular to a method for removing a bimetallic catalyst. Background Art

[0002] Double Metal Cyanide (DMC) catalysts play an important role in the synthesis of low-unsaturation high molecular weight polyethers due to their high efficiency. These polyethers are widely used in products such as soft foam polyethers, spinning oils, and PAG lubricants. However, in current industrial applications, catalysts are often not completely removed from the final product, which may bring some environmental and health risks.

[0003] DMC catalyst is usually in a heterogeneous system in polyether, and may separate and produce floccules during long-term storage, affecting the appearance and application performance of the product. More seriously, DMC catalyst may decompose under air oxidation, producing heavy metals such as cobalt and highly toxic cyanide, which are harmful to the environment and human health. With the increase of environmental awareness, these potential risks are receiving more and more attention. Summary of the invention

[0004] The technical problem to be solved by the present invention is to overcome the technical defects of the background technology and provide a method for removing the bimetallic catalyst. The raw materials of the present invention are easily available and the operation is simple. The residual DMC catalyst in the polyether polyol can be effectively removed, the purity and color of the product can be improved, and the influence of peroxide can be eliminated at the same time, which has significant environmental and economic benefits.

[0005] The technical solution adopted by the present invention to solve the above technical problems is as follows:

[0006] A method for removing a bimetallic catalyst comprises the following steps:

[0007] (1) mixing a polyether polyol containing a DMC catalyst with a hydrogen peroxide solution to form floccules;

[0008] (2) mixing the above polyether polyol with manganese dioxide and water for a certain period of time to remove peroxide;

[0009] (3) adding a filter aid, removing water, filtering insoluble matter, and obtaining a pure polyether polyol free of DMC catalyst.

[0010] In the above technical solution, in step (1), the DMC catalyst is a zinc-cobalt double metal cyanide complex catalyst.

[0011] Preferably, in step (1), the concentration of the hydrogen peroxide solution is 30% to 50%, and the added amount is 0.05% to 0.5% of the mass of the polyether polyol, more preferably 0.1% to 0.2%.

[0012] Preferably, in step (1), the mixing temperature of the polyether polyol and the hydrogen peroxide solution is 80 to 130° C., more preferably 100 to 110° C., and the mixing time is 1 to 2 hours.

[0013] Preferably, in step (2), the amount of manganese dioxide added is 0.01% to 0.1% of the mass of the polyether polyol in step (1), more preferably 0.05%.

[0014] Preferably, in step (2), the amount of water added is 0.2% to 5% of the mass of the polyether polyol in step (1).

[0015] Preferably, in step (2), the water is deionized water.

[0016] Preferably, in step (2), the mixing temperature of the polyether polyol and manganese dioxide is 100 to 140° C., and the mixing time is 2 to 6 hours.

[0017] Preferably, in step (3), the filter aid is a commonly used polyether adsorbent magnesium silicate or magnesium aluminum silicate.

[0018] Preferably, in step (3), the amount of the filter aid added is 0.1% to 0.3% of the mass of the polyether polyol in step (1).

[0019] Preferably, in step (3), the process for removing moisture is high-temperature vacuum negative pressure nitrogen dehydration, the temperature is 100 to 130° C., and the nitrogen pressure of the drum is -0.09 to -0.098 MPa.

[0020] Preferably, in step (3), the filtration process adopts plate and frame circulation filtration or filter paper filtration.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The invention has the characteristics of readily available raw materials, simple process, low cost and high efficiency; the polyether polyol after removal has high purity, low DMC catalyst residue and improved product color; in addition, through the use of manganese dioxide, peroxide is effectively decomposed, eliminating its potential influence in the subsequent polyurethane preparation process; through these technical improvements, the invention provides a practical solution for solving the problem of removing the polyether DMC catalyst, which is helpful to promote the green and sustainable development of polyether polyol production. DETAILED DESCRIPTION

[0023] In order to better understand the content of the present invention, further description is given below in conjunction with specific embodiments. It should be understood that these embodiments are only used to further illustrate the present invention, and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content described in the present invention, those skilled in the art make some non-essential changes or adjustments to the present invention, which still belong to the protection scope of the present invention.

[0024] Example 1

[0025] (1) Synthesis of Polyol A

[0026] 92 g of glycerol and 1.5 g of potassium hydroxide were added to the reaction kettle, and the temperature was raised to 120-130°C, and nitrogen was blown for degassing for 2 h. Then, 408 g of propylene oxide was continuously added at this temperature, and the pressure was controlled at about 0.2-0.3 MPa. After ripening, the mixture was neutralized with phosphoric acid, dehydrated and filtered to obtain intermediate 305 (molecular weight about 500).

[0027] 200g of intermediate 305 and 0.2g of DMC catalyst (Huaian Bader polyurethane, double metal cyanide complex catalyst) were heated to 120-130°C and degassed with nitrogen for 2h. Then, about 80g of propylene oxide was added, and after inducing the reaction at above 150°C, 1800g of propylene oxide was continuously added. After complete aging, polyol A (appearance: transparent liquid, hydroxyl value: 33.5mgKOH / g, color (PT-co): 25, moisture: 0.03%, containing 22.1ppm Zn and 13.3ppm cobalt) was obtained.

[0028] (2) Polyol A bimetallic removal

[0029] Heat 500g of polyol A to 90°C, add 0.5g of 50% hydrogen peroxide, mix and stir at 110°C for 1h; then add 0.1g of manganese dioxide and 25g of deionized water, mix and stir at 110°C for 6h; then add 1g of magnesium aluminum silicate (Zhejiang Jiehua New Materials Co., Ltd., JH600#), nitrogen blow at 120°C under a negative pressure of -0.095Mpa until the moisture content is less than 0.05%, add 10761g of antioxidant, filter with filter paper with a pore size of 100μm to obtain clarified polyol A (appearance: transparent liquid, hydroxyl value: 33.5mgKOH / g, color (PT-co): 25, moisture: 0.04%, containing Zn<1ppm, cobalt<1ppm).

[0030] Example 2

[0031] (1) Synthesis of Polyol B

[0032] 74 g of n-butanol and 0.4 g of potassium hydroxide were added to the reactor, and the temperature was raised to 130-150°C, and nitrogen was blown for degassing for 2 h. Then, 376 g of propylene oxide / ethylene oxide (mass ratio of about 50:50) was continuously added at this temperature, and the pressure was controlled at about 0.2-0.3 MPa. After aging, it was neutralized with phosphoric acid, dehydrated and filtered to obtain the intermediate B-400 (molecular weight of about 400).

[0033] 400g of intermediate B-400 and 0.1g of DMC catalyst (Shanghai Qike, double metal cyanide complex catalyst) were heated to 120-130°C and degassed with nitrogen for 2h. Then, about 80g of propylene oxide / ethylene oxide was added, and after inducing the reaction at above 150°C, 2020g of propylene oxide / ethylene oxide (mass ratio of about 50:50) was continuously added. After complete aging, polyol B was obtained (appearance: liquid containing a small amount of floccules after standing, hydroxyl value: 22.5mgKOH / g, color (PT-co): 15, moisture: 0.02%, containing 13.0ppm Zn and 7.2ppm cobalt).

[0034] (2) Polyol B bimetallic removal

[0035] Heat 500 g of polyol B to 120° C., add 0.3 g of 50% hydrogen peroxide, mix and stir at 120° C. for 1 h; then add 0.3 g of manganese dioxide and 5 g of deionized water, mix and stir at 120° C. for 4 h; then add 0.5 g of aluminum silicate (Zhejiang Jiehua New Materials Co., Ltd., JH700#), nitrogen is blown at 120° C. under a negative pressure of -0.098 MPa until the moisture content is less than 0.2%, and filter with filter paper with a pore size of 100 μm to obtain clarified polyol B (appearance: transparent liquid, hydroxyl value: 22.5 mgKOH / g, color (PT-co): 10, moisture: 0.02%, containing Zn<1 ppm, cobalt<1 ppm).

[0036] Example 3

[0037] (1) Synthesis of Polyol C

[0038] Add 76g of propylene glycol and 0.6g of potassium hydroxide to the reactor, heat to 130-150°C, and degas with nitrogen for 2h. Then, at this temperature, continuously add 524g of propylene oxide / ethylene oxide (mass ratio of about 30:70), control the pressure at about 0.2-0.3Mpa, and after complete aging, neutralize with phosphoric acid, dehydrate and filter to obtain the intermediate PG-600 (molecular weight of about 400).

[0039] 300g of intermediate PG-600 and 0.5g of DMC catalyst (Shanghai Qike, double metal cyanide complex catalyst) were heated to 120-130°C and degassed with nitrogen for 2h. Then, about 80g of propylene oxide / ethylene oxide was added, and after inducing the reaction at above 150°C, 2700g of propylene oxide / ethylene oxide (mass ratio of about 30:70) was continuously added. After complete aging, polyol C was obtained (appearance: liquid containing a small amount of floccules after standing, hydroxyl value: 18.5mgKOH / g, color (PT-co): 25, moisture: 0.02%, containing 36.7ppm Zn and 19.8ppm cobalt).

[0040] (2) Polyol C bimetallic removal

[0041] Heat 500 g of polyol C to 100° C., add 1 g of 50% hydrogen peroxide, mix and stir at 120° C. for 2 h; then add 0.5 g of manganese dioxide and 10 g of deionized water, mix and stir at 120° C. for 3 h; then add 1.5 g of aluminum silicate (Zhejiang Jiehua New Materials Co., Ltd., JH700#), blow nitrogen at 120° C. under a negative pressure of -0.095 MPa until the moisture content is less than 0.1%, filter, and obtain clarified polyol C (appearance: transparent liquid, hydroxyl value: 18.5 mgKOH / g, color (PT-co): 10, moisture: 0.04%, containing Zn<1 ppm), cobalt<1 ppm).

[0042] The above description is not intended to limit the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by a person skilled in the art within the spirit and scope of the present invention shall also fall within the protection scope of the present invention.

Claims

1. A method for removing a bimetallic catalyst, characterized in that: The steps include: (1) mixing a polyether polyol containing a DMC catalyst with a hydrogen peroxide solution to form floccules; (2) mixing the above polyether polyol with manganese dioxide and water for a certain period of time to remove peroxide; (3) adding a filter aid, removing water, filtering insoluble matter, and obtaining a pure polyether polyol free of DMC catalyst.

2. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (1), the concentration of the hydrogen peroxide solution is 30% to 50%, and the added amount is 0.05% to 0.5% of the mass of the polyether polyol.

3. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (1), the mixing temperature of the polyether polyol and the hydrogen peroxide solution is 80 to 130° C., and the mixing time is 1 to 2 hours.

4. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (2), the amount of manganese dioxide added is 0.01% to 0.1% of the mass of the polyether polyol in step (1).

5. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (2), the amount of water added is 0.2% to 5% of the mass of the polyether polyol in step (1).

6. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (2), the mixing temperature of the polyether polyol and manganese dioxide is 100 to 140° C., and the mixing time is 2 to 6 hours.

7. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (3), the filter aid is magnesium silicate or magnesium aluminum silicate.

8. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (3), the amount of the filter aid added is 0.1% to 0.3% of the mass of the polyether polyol in step (1).

9. A method for removing a bimetallic catalyst as claimed in claim 1, characterized in that: In step (3), the process for removing moisture is high-temperature vacuum negative pressure nitrogen drum dehydration, the temperature is 100 to 130° C., and the drum N2 pressure is -0.09 to -0.098 MPa.

10. The method for removing a bimetallic catalyst according to claim 1, characterized in that: In step (3), the filtration process adopts plate and frame circulation filtration or filter paper filtration.