Self-repairing fluorine-containing polyurethane and preparation method thereof
By introducing fluorine atoms into polyurethane and using its surface driving force to achieve entanglement and reconstruction of molecular chains, the problem of self-healing fluorine-containing polyurethane losing its repair ability in harsh environments is solved, and efficient physical self-repair and excellent Mechanical properties, suitable for industrial applications.
Patent Information
- Application Number
- CN202411211661.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-01
AI Technical Summary
The existing self-healing fluorine-containing polyurethane achieved by chemical methods loses its repair ability under organic solvents or harsh conditions, and physical repair methods are difficult to achieve excellent mechanical properties, which limits its industrial application.
By introducing fluorine atoms into polyurethanes of specific structural types, the properties of fluorine atoms being easily migrated to the surface can be used to achieve entanglement and reconstruction of molecular chains, and physical methods are used to self-heal at room temperature and heating environment to avoid chemical bond changes. The process is simple and the repair efficiency is high.
It achieves efficient self-repair under various solvent environments and extreme conditions, maintains repair efficiency of more than 80%, and has a simple design process, which is suitable for industrial production.
Smart Images

Figure CN118878784A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a self-repairing polyurethane material, in particular to a self-repairing fluorine-containing polyurethane and a preparation method thereof. Background Art
[0002] Among polymers, thermoplastic elastomers with soft and hard segment phase separation structures, especially elastomers with self-healing properties, have attracted widespread attention in wearable electronic devices, biomedicine, and defense industry due to their high performance and easy processing.
[0003] At present, there are two methods to make polymers self-repairing, namely chemical methods and physical methods. Chemical repair methods are the most commonly used methods, which mainly introduce reversible interactions such as dynamic reversible bonds or supramolecular interactions to achieve self-repair of polymers through efficient dynamic interactions. However, polymers that achieve self-repair through chemical methods are usually unable to be repaired in various extremely harsh environments, such as organic solvents, strong acid or strong alkali environments, redox agent environments, etc. This is because chemical bonds are easily destroyed by environmental conditions, thereby losing their post-reversibility. At this stage, there are two ways to solve this problem: one is to introduce multiple dynamic covalent bonds into the polymer to ensure that the polymer is stable in various environments, but this will increase the complexity of experimental design, increase costs, and is not conducive to industrial production; the other way is to achieve repair through physical methods. Unlike chemical repair methods, physical repair methods do not involve changes in chemical bonds. They only promote the diffusion, entanglement and redispersion of molecular chains through strong driving forces to restore mechanical properties. The entire process is less affected by the external environment, so it can be repaired in various extremely harsh environments. However, the materials repaired by this method usually have poor mechanical properties and are difficult to achieve industrial application. Moreover, physical repair methods can usually only be implemented in specific systems, such as polymers with specific molecular weights, and are not a universal repair method. Therefore, the development of polymer materials with excellent mechanical properties that can be repaired by physical methods is an urgent problem to be solved in the field of self-repair.
[0004] At present, there are many studies on self-healing fluorinated polyurethanes, but all of them achieve self-healing through chemical methods. These fluorinated polyurethanes will lose their repair ability in various organic solvents or harsh conditions. Summary of the invention
[0005] In view of the problem that the self-healing fluorinated polyurethane achieved by chemical methods will lose its repair ability in various organic solvents or harsh conditions, the present invention provides a self-healing fluorinated polyurethane and a preparation method thereof, which introduces fluorine atoms into polyurethane of a specific structural type to achieve self-healing of the material by physical methods without involving changes in chemical bonds, and has high repair efficiency.
[0006] In order to achieve the above object, the present invention provides a self-repairing fluorinated polyurethane having the following structure:
[0007]
[0008] Wherein, R1 is methyl, phenyl or vinyl, m is in the range of 6 to 20, n is in the range of 15 to 60, and w is in the range of 1 to 4.
[0009] The present invention introduces fluorine atoms into polyurethanes of a specific structural type and utilizes the property that fluorine atoms easily migrate to the surface, thereby improving the mobility of the molecular chains, facilitating the entanglement and reconstruction of the molecular chains at the incision. When the fluorinated polyurethane is cut, the polymer network will break. When the two newly cut surfaces come into contact under the action of an external force, driven by the surface free energy, the fluorinated chain segments close to the incision gradually diffuse to the incision surface, and this process can be accelerated by heating until the incision is completely restored. Subsequently, the fluorinated chain segments will be redispersed into the body of the fluorinated polyurethane to achieve equilibrium. During this back-and-forth motion of the polymer chains, the fluorinated chain segments penetrate each other, and the mechanical properties (such as Fig.15 The self-repair of the material is achieved through physical methods without involving changes in chemical bonds. The design process is simple and the repair efficiency is high. The mechanical properties of the polymer can also be regulated by adjusting the content of the introduced fluorinated diol.
[0010] The second aspect of the present invention provides a method for preparing the above-mentioned self-healing fluorinated polyurethane, the preparation method comprising the following steps:
[0011] S1, uniformly mixing a polymer polyol, a diisocyanate and a catalyst and reacting them to prepare a polyurethane prepolymer;
[0012] S2, adding a fluorinated diol as a chain extender to the polyurethane prepolymer obtained in step S1 at 40-70° C. to carry out a chain extension reaction to prepare a fluorinated polyurethane prepolymer;
[0013] S3, removing the solvent from the fluorinated polyurethane prepolymer obtained in step S2, and aging it to obtain the self-healing fluorinated polyurethane;
[0014] Among them, the raw material feeding formula is mainly related to two factors: R value and hard segment content. The calculation method is as follows:
[0015]
[0016] Taking into account the possible presence of trace amounts of water molecules in the air that may react with isocyanate, the R value is selected to be 0.92-1.02; in order to more easily regulate the mechanical properties of the fluorinated polyurethane, the hard segment content is selected to be 30%-50%, and the catalyst dosage is 3‰-5‰ of the total feed mass.
[0017] The above method is based on the method of preparing polyurethane in the prior art. By adopting fluorinated diols as chain extenders instead of traditional small molecule diols, fluorine atoms are introduced into polyurethanes of specific structural types to form fluorine-hydrogen bonds, thereby preparing a self-healing fluorinated polyurethane described in the present invention.
[0018] Among them, polymer polyol is a kind of polyester polyol and polyether polyol, and polymer polyol is mainly used as the soft segment in polyurethane.
[0019] Preferably, the polymer polyol is trihydroxy polyether (N330), polycaprolactone diol (PCL), polytetramethylene glycol (PTMG), polyethylene glycol (PEG) or bishydroxyalkyl-terminated polydimethylsiloxane, and the molecular weight is 500-6000.
[0020] The diisocyanate is one of hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate and diphenylmethane diisocyanate.
[0021] The catalyst is a catalyst commonly used in preparing polyurethane prepolymers, preferably dibutyltin dilaurate (DBTDL).
[0022] Specifically, in step S1, the polymer polyol is heated to 100-120°C and the water is removed under vacuum, then the temperature is lowered to 70-90°C, the diisocyanate and the catalyst are slowly added dropwise, and the reaction is performed for 1h-4h to prepare a polyurethane prepolymer containing an isocyanate group (-NCO). Preferably, the temperature is lowered to 70-80°C, the diisocyanate and the catalyst are slowly added dropwise, and the reaction is preferably stirred during the reaction, and the stirring time is preferably 2-4h, and most preferably 2-3h.
[0023] Preferably, the reaction process is carried out under an inert atmosphere to ensure that water molecules in the air do not enter the reaction container and interfere with the reaction.
[0024] Preferably, in step S2, the fluorinated diol is tetrafluorobutanediol, octafluorobutanediol, dodecafluorobutanediol or hexafluorobutanediol, and the concentration is 0.1-0.5 g / ml.
[0025] Preferably, in step S2, the chain extension reaction time is 2 to 3 hours.
[0026] Specifically, in step S3, the solvent is removed by reduced pressure distillation under vacuum, and then the self-healing fluorine-containing polyurethane is cured at 90 to 120° C. for 24 to 72 hours to obtain the self-healing fluorine-containing polyurethane.
[0027] On the basis of the above technical solution, after the chain extension reaction in step S2, a cross-linking agent or a small molecule diol with a concentration of 0.1 to 0.5 g / ml is added to the system, and the chain extension reaction is continued for 0.5 to 2 hours, preferably 0.5 to 1 hour. After the reaction is completed, a fluorinated polyurethane prepolymer is prepared. The use of a cross-linking agent or a small molecule diol to continue the chain extension reaction can improve the mechanical properties of the polyurethane.
[0028] Preferably, the crosslinking agent is trimethylolpropane, trimethylolisopropylmethane, trimethylolphenol or hexamethylolhexane, and the small molecule diol is 1,4-butanediol, ethylene glycol, 1,3-propylene glycol, 1,6-hexanediol or dimethylpropylene glycol.
[0029] The repair temperature of the fluorinated polyurethane is from room temperature to 100°C, preferably 50-80°C, and most preferably 70-80°C.
[0030] Through the above technical solution, the present invention achieves the following beneficial effects:
[0031] 1. The self-healing fluorine-containing polyurethane provided by the present invention introduces fluorine atoms into a polyurethane of a specific structural type, and utilizes the property that fluorine atoms can easily migrate to the surface. Driven by the surface free energy, the fluorine-containing chain segments gradually migrate from the inside of the incision to the incision. The surface free energy provided by the fluorine-containing component is the main driving force that enables the molecular chain to migrate rapidly, which is not possessed by other polymers repaired by physical methods. This strong driving force allows the fluorine-containing chain ends to migrate rapidly to the incision, where they diffuse, entangle and redisperse. Unlike traditional self-healing polyurethanes, there is no need to add other chemical bonds, and the repair process does not involve changes in chemical bonds. Self-healing can be achieved in a variety of solvent environments, and repair can be achieved by physical methods at room temperature and in heated environments. Self-healing can be achieved in various extreme environments.
[0032] 2. The present invention can adjust the content of the introduced fluorinated diol to achieve the regulation of the mechanical properties of the polymer. When the content of the fluorinated diol is reduced, the toughness of the self-healing fluorinated polyurethane will increase.
[0033] 3. In the preparation method of the self-healing fluorinated polyurethane of the present invention, a simple fluorinated diol small molecule is used as a fluorinated chain extender to obtain a fluorinated polyurethane elastomer with a self-healing effect. The design process is simple and does not introduce complex chemical bonds. At the same time, it can also be mass-produced to achieve industrialization.
[0034] 4. Since the self-healing fluorinated polyurethane of the present invention is repaired without reversible chemical bonds, it can maintain a repair efficiency of more than 80% in a variety of solvent environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Example 1 of the present invention;
[0036] Figure 2 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Example 1 of the present invention at 70°C;
[0037] Figure 3 This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Example 2 of the present invention;
[0038] Figure 4 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Example 2 of the present invention at 70°C;
[0039] Figure 5 This is a graph showing the repair performance of the self-healing fluorinated polyurethane prepared in Example 2 of the present invention under different environments;
[0040] Figure 6 This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Example 3 of the present invention;
[0041] Figure 7 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Example 3 of the present invention at 70°C;
[0042] Figure 8 This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Example 4 of the present invention;
[0043] Fig. 9 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Example 4 of the present invention at 70°C;
[0044] Fig.10 This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Example 5 of the present invention;
[0045] Fig.11 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Example 5 of the present invention at 70°C;
[0046] Fig.12 This is the infrared spectrum of the self-healing fluorinated polyurethane prepared in Comparative Example 1;
[0047] Fig.13 This is a graph of the mechanical properties of the self-healing fluorinated polyurethane prepared in Comparative Example 2 at 70°C;
[0048] Fig.14 The mechanical properties and repair performance diagram of the fluorinated polyurethane prepared in Comparative Example 2;
[0049] Fig.15 Schematic diagram of the present invention achieving repair through diffusion and entanglement of fluorinated chain segments. DETAILED DESCRIPTION
[0050] The specific implementation of the present invention is described in detail below in conjunction with the examples. It should be understood that the specific implementation described herein is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0051] In the following examples, the solvents used were all firstly distilled with calcium hydride to remove water before use, and the remaining raw materials were purchased from commercial channels and used directly.
[0052] Example 1
[0053] Polycaprolactone diol (8.0 g, molecular weight 2000) was added to a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C for 1 hour. Then the temperature was lowered to 80°C, and hexamethylene diisocyanate HMDI (2.6505 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (57 mg) were added to the three-necked flask. Under a nitrogen atmosphere, the mixture was stirred for 2 hours for pre-polymerization and end-capping.
[0054] After cooling to 70°C, the fluorinated chain extender tetrafluorobutanediol (0.5197 g, 0.1 g / ml) was dissolved in THF (tetrahydrofuran) solution. After it was completely dissolved, it was added to a three-necked flask and continued to stir and reflux for 2 hours. After the reaction was completed, the product was placed in an oven, and the THF solvent and bubbles were removed by vacuum, and nitrogen was introduced for protection. The curing reaction was allowed to cure in an oven at 110°C for 48 hours, then the sample was taken out and cooled to room temperature, and finally a fluorinated self-healing polyurethane film extended with tetrafluorobutanediol was obtained.
[0055] The chemical structure of the self-healing fluorinated polyurethane was characterized by infrared spectroscopy, such as Figure 1 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and the repairable fluorinated polyurethane was successfully synthesized.
[0056] According to the national standard GB / T 528-1998, fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Figure 2 It can be seen that the fluorine-containing polyurethane obtained in Example 1 has excellent repair performance, and both stress and strain can be completely restored.
[0057] Example 2
[0058] Polycaprolactone diol (8.0 g, molecular weight 2000) was added into a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C for 1 hour. Then the temperature was lowered to 80°C, and HMDI (2.6505 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (57 mg) were added into the three-necked flask. The mixture was stirred for 2 hours under a nitrogen atmosphere for pre-polymerization and end-capping.
[0059] After cooling to 70°C, the fluorinated chain extender tetrafluorobutanediol (0.5197g, 0.1g / ml) was dissolved in THF (tetrahydrofuran) solution. After it was completely dissolved, it was added to a three-necked flask and continued to stir and reflux for 2h. Then trimethylolpropane (0.2598g, 0.1g / ml) was dissolved in THF. After trimethylolpropane was completely dissolved, it was poured into a three-necked flask and continued to reflux and extend for 1h. After the reaction was completed, the product was placed in an oven, vacuumed to remove the THF solvent and bubbles, and nitrogen was introduced for protection. The curing reaction was cured in an oven at 110°C for 48h, and then the sample was taken out and cooled to room temperature. Finally, a fluorinated self-healing polyurethane film with tetrafluorobutanediol and trimethylolpropane chain extension was obtained.
[0060] The chemical structure of the self-healing fluorinated polyurethane was characterized by infrared spectroscopy, such as Figure 3 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and the repairable fluorinated polyurethane was successfully synthesized.
[0061] According to the national standard GB / T 528-1998, fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Figure 4 It can be seen that the fluorine-containing polyurethane obtained in Example 2 has excellent repair performance, and both stress and strain can be completely restored.
[0062] The fluorine-containing self-healing polyurethane prepared in this example was placed in different solvent environments to study the repair properties of the polyurethane. Figure 5 As shown, since the repair is not through reversible chemical bonds, the repair efficiency can be maintained at over 80% in a variety of solvent environments.
[0063] Example 3
[0064] Polytetrahydrofuran (8.17 g, molecular weight 2000) was added into a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C. Then the temperature was lowered to 70°C, and toluene diisocyanate (2.7581 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (58 mg) were added into the three-necked flask, and the mixture was stirred for 3 hours under a nitrogen atmosphere for pre-polymerization and end-capping.
[0065] After cooling to 60°C, the fluorinated chain extender tetrafluorobutanediol (0.3709 g, 0.5 g / ml) was dissolved in the THF solution. After it was completely dissolved, it was added to a three-necked flask and continued to stir and reflux for 2.5 hours. Then, 1,4-butanediol (0.3709 g, 0.5 g / ml) was dissolved in THF. After trimethylolpropane was completely dissolved, it was poured into the three-necked flask and continued to reflux and extend the chain for 1 hour. After the reaction was completed, the reaction solution was poured into a tetrafluoroethylene mold.
[0066] Finally, the reaction liquid was put into an oven, and after vacuuming to remove the THF solvent and bubbles, nitrogen was introduced for protection. The curing reaction was allowed to cure in an oven at 110°C for 60 hours, and then the sample was taken out and cooled to room temperature. Finally, a fluorinated self-healing polyurethane film with tetrafluorobutanediol and 1,4-butanediol chain extension was obtained.
[0067] The chemical structure of the self-healing fluorinated polyurethane was characterized by infrared spectroscopy, such as Figure 6 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and the repairable fluorinated polyurethane was successfully synthesized.
[0068] According to the national standard GB / T 528-1998, fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Figure 7 It can be seen that the fluorine-containing polyurethane obtained in Example 3 has excellent repair performance, and both stress and strain can be completely restored.
[0069] Example 4
[0070] Polydimethylsiloxane (6.0 g, molecular weight 550) was added to a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C. Then the temperature was lowered to 80°C, and isophorone diisocyanate (2.0595 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (57 mg) were added to the three-necked flask. Under a nitrogen atmosphere, the mixture was stirred for 2 hours for pre-polymerization and end-capping.
[0071] After cooling to 60°C, the fluorinated chain extender octafluorobutanediol (0.1707g, 0.3g / ml) was dissolved in the THF solution. After it was completely dissolved, it was added to a three-necked flask and continued to stir and reflux for 3h. Then trimethylolphenol (0.3404g, 0.3g / ml) was dissolved in THF. After the trimethylolphenol was completely dissolved, it was poured into a three-necked flask and continued to reflux and extend the chain for 1h. After the reaction was completed, the reaction solution was placed in an oven, and after vacuuming to remove the THF solvent and bubbles, nitrogen was introduced for protection. The curing reaction was cured in an oven at 120°C for 60h, and then the sample was taken out and cooled to room temperature. Finally, a fluorinated self-healing polyurethane film with octafluorobutanediol and trimethylolphenol chain extension was obtained.
[0072] The chemical structure of the self-healing fluorinated polyurethane was characterized by infrared spectroscopy, such as Figure 8 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and the repairable fluorinated polyurethane was successfully synthesized.
[0073] According to the national standard GB / T 528-1998, fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Fig. 9 It can be seen that the fluorine-containing polyurethane obtained in Example 4 has excellent repair performance, and both stress and strain can be completely restored.
[0074] Example 5
[0075] Polyethylene glycol (6.34 g, molecular weight 2000) was added into a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C. Then the temperature was lowered to 80°C, and toluene diisocyanate (2.1936 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (57 mg) were added into the three-necked flask, and the mixture was stirred for 3 hours under a nitrogen atmosphere for pre-polymerization and end-capping.
[0076] Then, the fluorinated chain extender dodecafluorobutanediol (0.1309 g, 0.5 g / ml) was dissolved in DMSO (dimethyl sulfoxide) solution, and after it was completely dissolved, it was added to a three-necked flask and continued to stir and reflux for 2.5 hours, and then the temperature was lowered to 70°C, and then hexanediol (0.3936 g) was dissolved in THF, mixed evenly, and poured into a three-necked flask to continue reflux and chain extension for 1 hour. After the reaction was completed, the reaction solution was poured into a polytetrafluoroethylene mold.
[0077] Finally, the polytetrafluoroethylene mold containing the reaction liquid was placed in an oven, and after vacuuming to remove the THF solvent and bubbles, nitrogen was introduced for protection. The curing reaction was allowed to cure in an oven at 100°C for 48 hours, and then the sample was taken out and cooled to room temperature. Finally, a fluorine-containing self-healing polyurethane film with dodecafluorobutanediol and hexanediol chain extension was obtained.
[0078] The chemical structure of the self-healing fluorinated polyurethane was characterized by infrared spectroscopy, such as Fig.10 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and the repairable fluorinated polyurethane was successfully synthesized.
[0079] According to the national standard GB / T 528-1998, fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Fig.11 It can be seen that the fluorinated polyurethane obtained in Example 5 has excellent repair performance, and both stress and strain can be completely restored.
[0080] Comparative Example 1
[0081] Polycaprolactone diol (10.04 g, molecular weight 2000) was added into a three-necked flask equipped with a stirring paddle, and the water was removed by vacuum at 120°C. Then the temperature was lowered to 80°C, and HMDI (2.6505 g) and 0.5% (mass fraction) of the total mass of the system catalyst DBTDL solution (65 mg) were added into the three-necked flask. Under a nitrogen atmosphere, the mixture was stirred for 3 hours for pre-polymerization and end-capping.
[0082] Then the temperature was lowered to 70°C, and 1,4-butanediol (0.2598 g, 0.5 g / ml) was dissolved in THF. After 1,4-butanediol was completely mixed, it was poured into a three-necked flask and refluxed for chain extension for 1 hour. After the reaction was completed, the reaction solution was poured into a PTFE mold.
[0083] Finally, the reaction solution was placed in an oven, and after vacuuming to remove the THF solvent and bubbles, nitrogen protection was introduced. The curing reaction was allowed to cure in an oven at 120°C for 48 hours, and then the sample was taken out and cooled to room temperature, and finally a polyurethane film with 1,4-butanediol chain extension was obtained.
[0084] The chemical structure of non-fluorinated polyurethanes was characterized by infrared spectroscopy, such as Fig.12 As shown, at 2250cm -1 No characteristic absorption peak of -CNO was found, indicating that the polymerization reaction was completed and non-fluorinated polyurethane was successfully synthesized.
[0085] According to the national standard GB / T 528-1998, non-fluorinated polyurethane was made into dumbbell-shaped specimens. At least 5 samples were prepared for each group. The sample thickness was about 2mm. The test was carried out at room temperature and the tensile rate was fixed at 100mm / min. A 1mm deep notch was pre-made in the middle of the dumbbell-shaped specimen. After repairing in an oven, the mechanical properties were tested by the universal tensile testing machine of Instron. The stress-strain curves before and after repair are shown in the figure. Fig.13 It can be seen that the non-fluorine-containing polyurethane obtained in Comparative Example 1 does not have repair performance, and both stress and strain cannot be restored.
[0086] Comparative Example 2
[0087] Take 6.00g PCL (Mn = 1000) in a 100mL three-necked flask and dehydrate it in a vacuum oven at 100℃ for 3h; add 2.68g HMDI under nitrogen protection, then add 0.024g DBTDL dissolved in 1mL THF, and react at 80℃ for 2h to obtain a polyurethane prepolymer. Add 0.913g fluorinated chain extender hexafluorobisphenol A, react at 45℃ for 1h to extend the chain; then add 2.11g 4-methylumbelliferone dissolved in 2mL DMF, react at 80℃ for 1h to cap the end; after the reaction, slowly pour the polyurethane product into the mold and cure at 80℃ for 24h. The mechanical properties and repair properties of fluorinated polyurethane are shown in Figure 2. Fig.14 Compared with the method of the embodiment of the present invention, only the type of fluorine-containing chain extender is changed, but the strain decreases significantly and cannot be completely repaired.
[0088] The preferred implementation modes of the present invention are described in detail above in combination with the embodiments; however, the present invention is not limited to the specific details in the above implementation modes. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical scheme of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0089] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0090] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a self-repairing fluorinated polyurethane, characterized in that: The steps include: S1, uniformly mixing a polymer polyol, a diisocyanate and a catalyst and reacting them to prepare a polyurethane prepolymer; S2, adding a fluorinated diol as a chain extender to the polyurethane prepolymer obtained in step S1 at 40-70° C. to carry out a chain extension reaction to prepare a fluorinated polyurethane prepolymer; S3, removing the solvent from the fluorinated polyurethane prepolymer obtained in step S2, and aging it to obtain the self-healing fluorinated polyurethane; The polymer polyol reacts to form the soft segment of the self-healing fluorinated polyurethane, and the diisocyanate reacts to form the hard segment of the self-healing fluorinated polyurethane. The raw material feed ratio meets the following requirements: R is 0.92-1.02, the hard segment content is 30%-50%, and the catalyst dosage is 3‰-5‰ of the total feed mass, wherein:
2. The method for preparing the self-repairing fluorinated polyurethane according to claim 1, characterized in that: In step S1, the polymer polyol is trihydroxy polyether, polycaprolactone diol, polytetramethylene glycol, polyethylene glycol or dihydroxyalkyl-terminated polydimethylsiloxane, and the molecular weight is 500-6000; the diisocyanate is hexamethylene diisocyanate, toluene diisocyanate, isophorone diisocyanate or diphenylmethane diisocyanate; and the catalyst is dibutyltin dilaurate.
3. The method for preparing the self-repairing fluorinated polyurethane according to claim 1, characterized in that: In step S1, the polymer polyol is heated to 100-120° C. and the moisture is removed under vacuum, then the temperature is lowered to 70-90° C., the diisocyanate and the catalyst are slowly added dropwise, and the reaction is carried out for 1-4 hours to prepare a polyurethane prepolymer containing an isocyanate group.
4. The method for preparing the self-repairing fluorinated polyurethane according to claim 3, characterized in that: The reaction process was carried out under an inert atmosphere.
5. The method for preparing the self-repairing fluorinated polyurethane according to claim 1, characterized in that: In step S2, the fluorine-containing diol is tetrafluorobutanediol, octafluorobutanediol, dodecafluorobutanediol or hexafluorobutanediol, and the concentration is 0.1-0.5 g / ml.
6. The method for preparing the self-repairing fluorinated polyurethane according to claim 1, characterized in that: In step S2, the chain extension reaction time is 2 to 3 hours.
7. The method for preparing the self-repairing fluorinated polyurethane according to claim 1, characterized in that: In step S3, the solvent is removed by reduced pressure distillation under vacuum, and then the self-healing fluorine-containing polyurethane is cured at 90 to 120° C. for 24 to 72 hours to obtain the self-healing fluorine-containing polyurethane.
8. The method for preparing the self-healing fluorinated polyurethane according to any one of claims 1 to 7, characterized in that: After the chain extension reaction in step S2, a cross-linking agent or a small molecule diol with a concentration of 0.1 to 0.5 g / ml is added to the system, and the chain extension reaction is continued for 0.5 to 2 hours. After the reaction is completed, a fluorine-containing polyurethane prepolymer is prepared.
9. The method for preparing the self-repairing fluorinated polyurethane according to claim 8, characterized in that: The cross-linking agent is trimethylolpropane, trimethylolisopropylmethane, trimethylolphenol or hexamethylolhexane, and the small molecule diol is 1,4-butanediol, ethylene glycol, 1,3-propylene glycol, 1,6-hexanediol or dimethylpropylene glycol.
10. A self-repairing fluorinated polyurethane, characterized in that: It is prepared by the preparation method described in any one of claims 1 to 9 and has the following structure: Wherein, R1 is methyl, phenyl or vinyl, m is in the range of 6 to 20, n is in the range of 15 to 60, and w is in the range of 1 to 4.
Citation Information
Patent Citations
High-strength high-toughness fluorine-containing polyurethane and preparation method thereof
CN113121788A
High-strength self-healing polyurethane polymer having room-temperature self-healing function
WO2022169317A1
Cited By
Polyurethane material with ionic interaction and preparation method thereof
CN119431721A
Wear-resistant and scratch-resistant leather and preparation method thereof
CN120484670A
Polyurethane-based rotary blowout preventer rubber core material and preparation method thereof
CN120944170A
Energy-containing self-repairing functional polyurethane and preparation method thereof
CN122520882A