Cloth pattern urea formaldehyde button and preparation method thereof

Through the specific process treatment and component combination of the resin masterbatch, the problem of the stiff feel of existing cloth buttons has been solved, and cloth-grained urea-formaldehyde buttons with clear fabric lines and good texture have been achieved, satisfying customers' environmentally friendly vision and texture. need.

CN118755233APending Publication Date: 2024-10-11ZHEJIANG WEIXING IND DEV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410883072.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Due to the material reasons, existing cloth-covered buttons have a stiff surface feel and lack the texture of fabric fibers, making them unable to meet customers' environmentally friendly visual and textural needs.

Method used

The resin masterbatch is used through extrusion, cutting, drying, hot pressing, polishing, soaking texturing, pH adjustment and drying, combined with melamine modified urea-formaldehyde resin, carboxymethyl cellulose and polyester filament, and is heated through The pressure causes the resin to liquefy and penetrate into the fabric, increasing the adhesion fastness and velvety, and improving the fabric texture of the buttons.

Benefits of technology

It achieves clear fabric texture and good fabric texture of cloth-grained urea-formaldehyde buttons, improves the water resistance and washing resistance of buttons, and meets customers' environmentally friendly visual and texture needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004925822160000011
    Figure BDA0004925822160000011
  • Figure BDA0004925822160000021
    Figure BDA0004925822160000021
  • Figure BDA0004925822160000031
    Figure BDA0004925822160000031
Patent Text Reader

Abstract

The invention belongs to the technical field of button production, and particularly relates to a woven urea formaldehyde button and a preparation method thereof. The woven urea-formaldehyde button provided by the invention is prepared by performing sheet extrusion, blank cutting, blank baking, cloth spreading and hot pressing, polishing, soaking and texturing, pH value adjustment, cleaning and drying on a resin master batch. The resin master batch is prepared from melamine modified urea resin, polyester yarns, sodium bicarbonate, carboxymethylcellulose, a lubricant and urotropine. The woven urea-formaldehyde button is mainly prepared from the melamine modified urea-formaldehyde resin, the carboxymethyl cellulose, the polyester silk and the fabric, due to the hot pressing effect, the melamine modified urea-formaldehyde resin is liquefied, flows and permeates into the fabric, so that the excellent bonding fastness is achieved, the fabric exists on the surface of the button, and the button has the texture of the same fabric; meanwhile, the carboxymethyl cellulose and the polyester yarns added into the resin master batch can be exposed from the interior of the urea resin after being subjected to the soaking and texturing process, so that the fabric texture of the surface of the button is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of button production, and in particular relates to a cloth-patterned urea-formaldehyde button and a preparation method thereof. Background Art

[0002] Buttons are one of the most common clothing accessories. They are the fastening materials of clothing and were originally used to connect the lapels of clothes. With the improvement of living standards, in addition to maintaining their original functions, they have gradually developed into a more artistic and decorative representative.

[0003] The buttons on the market are mostly made of metal, thermoplastics, thermosetting resins, fruits, horns, bones, shells, etc. With the rise of Recycle, Reuse, Reduce, Replace at home and abroad, customers' demand for environmental friendliness is increasing. Among them, fabric buttons, as a visually visible recyclable concept button, have a versatile effect with fabrics and are deeply loved by customers.

[0004] Generally, cloth-effect buttons are made by spreading a layer of transparent unsaturated polyester resin on a centrifuge, and then spreading the fabric after the glue is removed, and then pouring another layer of unsaturated polyester resin to obtain a button that looks like a visible fabric. However, due to the material, the surface feels stiff and plastic-like, and does not have the texture of fabric fibers. Summary of the invention

[0005] In view of this, an object of the present invention is to provide a cloth-textured urea-formaldehyde button and a preparation method thereof. The cloth-textured urea-formaldehyde button prepared by the present invention has clear fabric texture and good fabric texture.

[0006] The present invention provides a cloth-patterned urea-formaldehyde button, which is made from a resin masterbatch through extrusion, embryo cutting, embryo baking, cloth application and hot pressing, polishing, soaking and roughening, pH value adjustment, cleaning and drying; the components of the resin masterbatch include, by weight:

[0007]

[0008]

[0009] Preferably, the melting point of the polyester yarn is 160-180°C.

[0010] Preferably, the degree of substitution of the carboxymethyl cellulose is 0.4 to 1.2.

[0011] Preferably, the lubricant is cyclohexyl stearate and / or glyceryl stearate.

[0012] Preferably, the resin masterbatch further comprises a pigment.

[0013] Preferably, the components of the treatment liquid used for soaking and texturing include, by weight:

[0014] 100 parts water;

[0015] 0.1-0.5 parts of polyoxyethylene sorbitan monostearate;

[0016] 5 to 10 parts of inorganic acid.

[0017] The present invention provides a method for preparing the cloth-patterned urea-formaldehyde buttons described in the above technical solution, comprising the following steps:

[0018] Extruding the resin masterbatch into sheets to obtain a sheet;

[0019] Cutting the sheet into blanks, and then drying to obtain dry blanks;

[0020] Laying fabric on the surface of the dried blank, followed by hot pressing to obtain a button blank;

[0021] polishing the button embryo to obtain a polished button embryo;

[0022] The polished button blank is immersed in a treatment liquid for hairening, and then the pH value is adjusted, washed and dried to obtain a cloth-textured urea-formaldehyde button.

[0023] Preferably, the temperature of the hot pressing molding is 140-150° C.; the pressure of the hot pressing molding is 10-20 mPa; and the time of the hot pressing molding is 60-180 s.

[0024] Preferably, the temperature of the soaking and texturing is 30-50° C.; and the time of the soaking and texturing is 5-10 minutes.

[0025] Preferably, the pH value is adjusted to 7-7.5.

[0026] Compared with the prior art, the present invention provides a cloth-patterned urea-formaldehyde button and a preparation method thereof. The cloth-patterned urea-formaldehyde button provided by the present invention is made from a resin masterbatch through extrusion, embryo cutting, embryo baking, cloth application and hot pressing, polishing, soaking and hairening, pH value adjustment, cleaning and drying; in parts by weight, the components of the resin masterbatch include: 40 to 60 parts of melamine-modified urea-formaldehyde resin, 5 to 10 parts of polyester yarn, 0.5 to 2 parts of sodium bicarbonate, 15 to 30 parts of carboxymethyl cellulose, 0.1 to 2 parts of lubricant, and 0.2 to 2 parts of methenamine. The cloth-textured urea-formaldehyde buttons provided by the present invention are mainly made of melamine-modified urea-formaldehyde resin, carboxymethyl cellulose, polyester yarn and fabric. Due to the effect of heat pressing, the melamine-modified urea-formaldehyde resin liquefies and flows and penetrates into the fabric to achieve excellent bonding strength, and the fabric exists on the surface of the button, so that the button has the same texture as the fabric; at the same time, the carboxymethyl cellulose and polyester yarn added to the resin masterbatch will be exposed from the inside of the urea-formaldehyde resin after the soaking and woolening process, which can increase the velvet on the button surface and further improve the fabric texture on the button surface. DETAILED DESCRIPTION

[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] The present invention provides a cloth-patterned urea-formaldehyde button, which is made from a resin masterbatch through extrusion, embryo cutting, embryo baking, cloth-applying vulcanization, polishing, soaking and roughening, pH value adjustment, cleaning and drying; the resin masterbatch comprises the following components in parts by weight:

[0029]

[0030] In the cloth-textured urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the melamine-modified urea-formaldehyde resin is the main adhesive; the melamine-modified urea-formaldehyde resin adopts the melamine-modified urea-formaldehyde resin purchased on the market; the content of the melamine-modified urea-formaldehyde resin in the resin masterbatch can specifically be 40 parts by weight, 41 parts by weight, 42 parts by weight, 43 parts by weight, 44 parts by weight, 45 parts by weight, 46 parts by weight, 47 parts by weight, 48 parts by weight, 49 parts by weight, 50 parts by weight, 51 parts by weight, 52 parts by weight, 53 parts by weight, 54 parts by weight, 55 parts by weight, 56 parts by weight, 57 parts by weight, 58 parts by weight, 59 parts by weight or 60 parts by weight.

[0031] In the cloth-grained urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the polyester yarn is an effect filler, which is resistant to acid and alkali, corrosion-resistant, and has strong toughness, and retains the fiber effect after being soaked and hairened; the melting point of the polyester yarn is preferably 160-180°C, and can be specifically 160°C, 161°C, 162°C, 163°C, 164°C, 165°C, 166°C, 167°C, 168°C, 169°C, 170°C, 171°C, 172°C, 173°C, 174°C, 175°C, 176°C, 177°C, 178°C, 179°C or 180°C; the content of the polyester yarn in the resin masterbatch can be specifically 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight or 10 parts by weight.

[0032] In the cloth-textured urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the sodium bicarbonate can generate fine bubbles when heated during molding, so that the buttons can achieve a more obvious roughening effect after being soaked and roughened; the sodium bicarbonate is preferably commercially available AR analytical pure sodium bicarbonate; the content of the sodium bicarbonate in the resin masterbatch can specifically be 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight or 2 parts by weight.

[0033] In the cloth-textured urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the carboxymethyl cellulose is used as an effect filler and enhances the water resistance of the finished buttons; the degree of substitution of the carboxymethyl cellulose is preferably 0.4-1.2, specifically 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.1 or 1.2; the content of the carboxymethyl cellulose in the resin masterbatch can specifically be 15 parts by weight, 16 parts by weight, 17 parts by weight, 18 parts by weight, 19 parts by weight, 20 parts by weight, 21 parts by weight, 22 parts by weight, 23 parts by weight, 24 parts by weight, 25 parts by weight, 26 parts by weight, 27 parts by weight, 28 parts by weight, 29 parts by weight or 30 parts by weight.

[0034] In the cloth-grained urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the lubricant can improve the fluidity during pressing, so that the urea-formaldehyde resin can penetrate into the fabric more easily; the lubricant is preferably cyclohexyl stearate and / or glyceryl stearate; the content of the lubricant in the resin masterbatch can specifically be 0.1 parts by weight, 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight or 2 parts by weight.

[0035] In the cloth-grained urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the urotropine is a stabilizer to neutralize the acidic substances slowly released during the preparation of the buttons; the content of the urotropine in the resin masterbatch can specifically be 0.2 parts by weight, 0.3 parts by weight, 0.4 parts by weight, 0.5 parts by weight, 0.6 parts by weight, 0.7 parts by weight, 0.8 parts by weight, 0.9 parts by weight, 1 part by weight, 1.1 parts by weight, 1.2 parts by weight, 1.3 parts by weight, 1.4 parts by weight, 1.5 parts by weight, 1.6 parts by weight, 1.7 parts by weight, 1.8 parts by weight, 1.9 parts by weight or 2 parts by weight.

[0036] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, in the resin masterbatch, the components of the resin masterbatch preferably also include pigments, and the type and amount of the pigments are determined according to customer needs. In the specific embodiment provided by the present invention, the pigments include but are not limited to titanium dioxide; the content of the pigments in the resin masterbatch is preferably 1 to 5 parts by weight, specifically 1 part by weight, 1.5 parts by weight, 2 parts by weight, 2.5 parts by weight, 3 parts by weight, 3.5 parts by weight, 4 parts by weight, 4.5 parts by weight or 5 parts by weight.

[0037] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, the baking temperature is preferably 40-50°C, specifically 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C; the baking time is preferably 12-24h, specifically 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0038] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, the hot pressing temperature of the cloth hot pressing is preferably 140-150°C, specifically 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C or 150°C; the hot pressing pressure of the cloth hot pressing is preferably 10-20mPa, specifically 10mPa, 11mPa, 12mPa, 13mPa, 14mPa, 15mPa, 16mPa, 17mPa, 18mPa, 19mPa or 20mPa; the hot pressing time of the cloth hot pressing is preferably 60-180s, specifically 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, 160s, 170s or 180s.

[0039] In the cloth-textured urea-formaldehyde button provided by the present invention, the soaking and texturizing requires the use of a treatment liquid, which can react with the urea-formaldehyde resin on the surface of the button blank, thereby exposing the fibers inside the button blank; the treatment liquid is preferably an acid solution with an active agent added, and its components preferably include, by weight:

[0040] 100 parts water;

[0041] 0.1-0.5 parts of active agent;

[0042] 5 to 10 parts of inorganic acid.

[0043] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, in the treatment liquid, the active agent is preferably polyoxyethylene sorbitan monostearate; the content of the active agent in the treatment liquid can specifically be 0.1 parts by weight, 0.15 parts by weight, 0.2 parts by weight, 0.25 parts by weight, 0.3 parts by weight, 0.35 parts by weight, 0.4 parts by weight, 0.45 parts by weight or 0.5 parts by weight.

[0044] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, in the treatment liquid, the inorganic acid is preferably hydrochloric acid; the content of the inorganic acid in the treatment liquid can specifically be 5 parts by weight, 5.5 parts by weight, 6 parts by weight, 6.5 parts by weight, 7 parts by weight, 7.5 parts by weight, 8 parts by weight, 8.5 parts by weight, 9 parts by weight, 9.5 parts by weight or 10 parts by weight.

[0045] In the cloth-textured urea-formaldehyde buttons provided by the present invention, the temperature for immersion and texturization is preferably 30-50°C, specifically 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C; the time for immersion and texturization is preferably 5-10min, specifically 5min, 5.5min, 6min, 6.5min, 7min, 7.5min, 8min, 8.5min, 9min, 9.5min or 10min.

[0046] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, the pH value is preferably adjusted to 7 to 7.5, specifically 7, 7.05, 7.1, 7.15, 7.2, 7.25, 7.3, 7.35, 7.4, 7.45 or 7.5.

[0047] In the cloth-patterned urea-formaldehyde buttons provided by the present invention, the drying method is preferably air-drying.

[0048] The present invention also provides a method for preparing the cloth-patterned urea-formaldehyde buttons described in the above technical solution, comprising the following steps:

[0049] Extruding the resin masterbatch into sheets to obtain a sheet;

[0050] Cutting the sheet into blanks, and then drying to obtain dry blanks;

[0051] Laying fabric on the surface of the dried blank, followed by hot pressing to obtain a button blank;

[0052] polishing the button embryo to obtain a polished button embryo;

[0053] The polished button blank is immersed in a treatment liquid for hairening, and then the pH value is adjusted, washed and dried to obtain a cloth-textured urea-formaldehyde button.

[0054] In the preparation method provided by the present invention, the components of the resin masterbatch and the treatment liquid have been introduced above and will not be repeated here.

[0055] In the preparation method provided by the present invention, the drying temperature is preferably 40-50°C, specifically 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C; the drying time is preferably 12-24h, specifically 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h or 24h.

[0056] In the preparation method provided by the present invention, the temperature of the hot pressing molding is preferably 140-150°C, specifically 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C or 150°C; the pressure of the hot pressing molding is preferably 10-20mPa, specifically 10mPa, 11mPa, 12mPa, 13mPa, 14mPa, 15mPa, 16mPa, 17mPa, 18mPa, 19mPa or 20mPa; the time of the hot pressing molding is preferably 60-180s, specifically 60s, 70s, 80s, 90s, 100s, 110s, 120s, 130s, 140s, 150s, 160s, 170s or 180s.

[0057] In the preparation method provided by the present invention, the soaking and texturing temperature is preferably 30-50°C, specifically 30°C, 31°C, 32°C, 33°C, 34°C, 35°C, 36°C, 37°C, 38°C, 39°C, 40°C, 41°C, 42°C, 43°C, 44°C, 45°C, 46°C, 47°C, 48°C, 49°C or 50°C; the soaking and texturing time is preferably 5-10min, specifically 5min, 5.5min, 6min, 6.5min, 7min, 7.5min, 8min, 8.5min, 9min, 9.5min or 10min.

[0058] In the preparation method provided by the present invention, the pH value is preferably adjusted to 7-7.5, specifically 7, 7.05, 7.1, 7.15, 7.2, 7.25, 7.3, 7.35, 7.4, 7.45 or 7.5.

[0059] In the preparation method provided by the present invention, the drying method is preferably air-drying.

[0060] The cloth-textured urea-formaldehyde buttons provided by the present invention are mainly made of melamine-modified urea-formaldehyde resin, carboxymethyl cellulose, polyester yarn and fabric. Due to the effect of heat pressing, the melamine-modified urea-formaldehyde resin liquefies and flows and penetrates into the fabric to achieve excellent bonding strength, and the fabric exists on the surface of the button, so that the button has the same texture as the fabric; at the same time, the carboxymethyl cellulose and polyester yarn added to the resin masterbatch will be exposed from the inside of the urea-formaldehyde resin after the soaking and woolening process, which can increase the velvet on the button surface and further improve the fabric texture on the button surface.

[0061] For the purpose of greater clarity, the present invention is described in detail with reference to the following examples and comparative examples.

[0062] In the following embodiments and comparative examples of the present invention, the melamine-modified urea-formaldehyde resin used is purchased from the market, specifically the melamine-modified urea-formaldehyde resin model HY654654 produced by Haoyao New Materials; the polyester yarn used is a filamentous polyester fiber with a melting point of 160 to 180° C.; the sodium bicarbonate used is AR analytical pure sodium bicarbonate; and the degree of substitution of the carboxymethyl cellulose used is 0.8.

[0063] Example 1

[0064] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0065]

[0066] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0067] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0068] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 20mPa, and the time is 120s;

[0069] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0070] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0071] Water 100 parts by weight;

[0072] 0.2 parts by weight of polyoxyethylene sorbitan monostearate;

[0073] 10 parts by weight of hydrochloric acid;

[0074] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50° C. for 5 minutes to make the button embryo surface hairy to achieve the desired effect; then use 5% sodium hydroxide solution to adjust the pH to 7.0-7.5, and then wash with clean water;

[0075] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0076] Example 2

[0077] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0078]

[0079] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0080] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0081] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 10mPa, and the time is 120s;

[0082] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0083] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0084] Water 100 parts by weight;

[0085] 0.2 parts by weight of polyoxyethylene sorbitan monostearate;

[0086] 5 parts by weight of hydrochloric acid;

[0087] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50° C. for 5 minutes to make the button embryo surface hairy to achieve the desired effect; then use 5% sodium hydroxide solution to adjust the pH to 7.0-7.5, and then wash with clean water;

[0088] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0089] Example 3

[0090] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0091]

[0092] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0093] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0094] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 15mPa, and the time is 120s;

[0095] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0096] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0097] Water 100 parts by weight;

[0098] 0.3 parts by weight of polyoxyethylene sorbitan monostearate;

[0099] 10 parts by weight of hydrochloric acid;

[0100] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50° C. for 5 minutes to make the button embryo surface hairy to achieve the desired effect; then use 5% sodium hydroxide solution to adjust the pH to 7.0-7.5, and then wash with clean water;

[0101] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0102] Comparative Example 1

[0103] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0104]

[0105] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0106] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0107] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 15mPa, and the time is 120s;

[0108] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0109] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0110] Water 100 parts by weight;

[0111] 0.2 parts by weight of polyoxyethylene sorbitan monostearate;

[0112] 10 parts by weight of hydrochloric acid;

[0113] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50°C for 5 minutes; then adjust the pH to 7.0-7.5 with 5% sodium hydroxide solution, and then wash with clean water;

[0114] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0115] Comparative Example 2

[0116] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0117]

[0118] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0119] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0120] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 20mPa, and the time is 120s;

[0121] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0122] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0123] Water 100 parts by weight;

[0124] 0.2 parts by weight of polyoxyethylene sorbitan monostearate;

[0125] 10 parts by weight of hydrochloric acid;

[0126] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50°C for 5 minutes; then adjust the pH to 7.0-7.5 with 5% sodium hydroxide solution, and then wash with clean water;

[0127] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0128] Comparative Example 3

[0129] Step 1: Prepare urea-formaldehyde resin masterbatch. The formula is as follows:

[0130]

[0131] Step 2: Put the above raw materials into a blender, mix them evenly, and then put them into a tablet extruder to extrude them into tablets;

[0132] Step 3: Put the above sheet into a blank cutter, cut it into blanks, and then put it into an oven for pre-drying at 50°C for 12 hours;

[0133] Step 4: Put the dried blank into the vulcanizer, lay the fabric required by the customer on the blank, and heat press it to form a button blank; wherein the hot pressing temperature is 145°C, the pressure is 20mPa, and the time is 120s;

[0134] Step 5: removing the button embryo and polishing it to obtain a polished button embryo;

[0135] Step 6: Prepare the post-treatment solution and heat it to 50°C. The formula is as follows:

[0136] Water 100 parts by weight;

[0137] 0.2 parts by weight of polyoxyethylene sorbitan monostearate;

[0138] 10 parts by weight of hydrochloric acid;

[0139] Step 7: Place the button embryo in the post-treatment solution of step 6 and soak at 50°C for 5 minutes; then adjust the pH to 7.0-7.5 with 5% sodium hydroxide solution, and then wash with clean water;

[0140] Step 8: Dry the buttons to obtain the cloth-textured urea-formaldehyde button products.

[0141] Effect evaluation

[0142] The cloth-patterned urea-formaldehyde button products prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested according to the international standards of ISO 105-C06-2010 "Color fastness to domestic and commercial washing", ISO 105-D01-2010 "Color fastness of textiles to dry cleaning", and ISO 105-X11-1994 "Color fastness of textiles to hot pressing", and their surface effects were observed. The results are shown in the following table:

[0143] Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Surface Effects Strong velvet feel Strong velvet feel Strong velvet feel Weak velvet feel Weak velvet feel Strong velvet feel Color fastness to washing Level 4.0 Level 4.0 Level 4.0 Level 4.0 Level 4.0 damaged Color fastness to dry cleaning Level 4.0 Level 4.0 Level 4.0 Level 4.0 Level 4.0 damaged Ironing color fastness Level 4.0 Level 4.0 Level 4.0 Level 4.0 Level 4.0 Level 4.0

[0144] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A cloth-textured urea-formaldehyde button, characterized in that: The resin masterbatch is prepared by extruding sheets, cutting embryos, baking embryos, applying cloth and hot pressing, polishing, soaking and roughening, adjusting pH value, cleaning and drying; the components of the resin masterbatch include, by weight:

2. The cloth-patterned urea-formaldehyde button according to claim 1, characterized in that: The melting point of the polyester yarn is 160-180°C.

3. The cloth-patterned urea-formaldehyde button according to claim 1, characterized in that: The degree of substitution of the carboxymethyl cellulose is 0.4 to 1.

2.

4. The cloth-patterned urea-formaldehyde button according to claim 1, characterized in that: The lubricant is cyclohexyl stearate and / or glyceryl stearate.

5. The cloth-patterned urea-formaldehyde button according to claim 1, characterized in that: The resin masterbatch also includes pigments.

6. The cloth-patterned urea-formaldehyde button according to claim 1, characterized in that: The components of the treatment liquid used for soaking and texturing include, by weight: 100 parts water; 0.1-0.5 parts of polyoxyethylene sorbitan monostearate; 5 to 10 parts of inorganic acid.

7. A method for preparing the cloth-patterned urea-formaldehyde buttons according to any one of claims 1 to 6, characterized in that: The following steps are involved: Extruding the resin masterbatch into sheets to obtain a sheet; Cutting the sheet into blanks, and then drying to obtain dry blanks; Laying fabric on the surface of the dried blank, followed by hot pressing to obtain a button blank; polishing the button embryo to obtain a polished button embryo; The polished button blank is immersed in a treatment liquid for hairening, and then the pH value is adjusted, washed and dried to obtain a cloth-textured urea-formaldehyde button.

8. The preparation method according to claim 7, characterized in that: The temperature of the hot pressing molding is 140-150° C.; the pressure of the hot pressing molding is 10-20 mPa; and the time of the hot pressing molding is 60-180 seconds.

9. The preparation method according to claim 7, characterized in that: The temperature of the soaking and texturing is 30-50° C.; the time of the soaking and texturing is 5-10 minutes.

10. The preparation method according to claim 7, characterized in that: The pH value is adjusted to 7-7.5.

Citation Information

Cited By

  • High-temperature-resistant flame-retardant molded button and manufacturing process thereof

    CN120535899A