Intrinsic flame-retardant organic silicon elastic foam as well as preparation method and application thereof
Through the reaction of side-active polysiloxane and hydrogen-containing polysiloxane and the method of forming cross-linking bonds with end-active polysiloxane, the problem of silicone foam being easily ignited in high-temperature environments is solved, and no need to add flame retardant is achieved. The intrinsic flame retardant silicone elastic foam of the agent has good flame retardant properties and environmental protection characteristics, and is suitable for closed environments.
Patent Information
- Application Number
- CN202410997600.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing silicone foams are easily ignited in high-temperature environments or under flame attack. Flame-retardant modification methods have problems of limited effectiveness and high cost, and cannot meet the high flame-retardant requirements of closed environments such as aerospace and aviation.
Foaming is achieved through the reaction of side-active polysiloxane and hydrogen-containing polysiloxane to generate gas, and cross-linking bonds are formed through the terminal-active polysiloxane to control the cross-link density to retain foam elasticity and improve flame retardant properties. Using the combined preparation method of component A and component B, there is no need to add flame retardants.
It has realized the intrinsic flame-retardant silicone elastic foam without adding flame retardant. It has the advantages of good flame-retardant performance, rapid speed, light weight, halogen-free, environmental protection and non-flammability. It is suitable for airtight environments such as aviation, aerospace and high-speed rail carriages.
Smart Images

Figure BDA0004960679910000031 
Figure BDA0004960679910000032 
Figure BDA0004960679910000041
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organosilicon materials, and more particularly to an intrinsic flame-retardant organosilicon elastic foam and a preparation method and application thereof. Background Art
[0002] Closed environments such as spacecraft, aircraft and high-speed rail carriages require the use of materials with higher flame retardant properties. For example, the flame retardant requirements of seat elastic foam materials must meet the TB / T3237 requirements and reach the levels of non-flammable, difficult to burn and extremely difficult to burn. At the same time, very high requirements are placed on smoke density, smoke toxicity and flame propagation. The commonly used flame retardant polyurethane foams cannot meet the standard requirements and cannot guarantee the safety of astronauts and other passengers. Therefore, it is very necessary to develop a new type of flame-retardant, low-smoke and non-toxic silicone foam. This material can also be used in other fields or application scenarios such as new energy vehicles and power storage stations, and building wire pipe sealing, and has broad application prospects.
[0003] Conventional silicone foam is prepared from hydrogenated polysiloxane, vinyl polysiloxane and terminal hydroxyl polysiloxane with high binding energy Si-O-Si skeleton, wherein hydrogenated polysiloxane containing Si-H undergoes silylation reaction with vinyl to produce crosslinks between chains, while Si-OH of terminal hydroxyl polysiloxane undergoes dehydrogenation condensation reaction with Si-H to produce hydrogen, thus achieving internal crosslinking and foaming to prepare silicone foam. The foam itself has the characteristics of low density, high chemical resistance, wide operating temperature range, flexibility and heat insulation, which makes it widely used in building materials, transportation and electrical applications. However, the side chain organic groups of linear polydimethylsiloxane (PDMS) chains are easily ignited when exposed to high temperature environment or flame attack, which seriously limits its application.
[0004] At present, most of the flame retardant modification methods of silicone foam are to add flame retardants for flame retardancy, such as adding inorganic flame retardants (aluminum hydroxide, magnesium hydroxide, calcium carbonate, etc.) and carbon flame retardants (graphite, graphene oxide, etc.). The large amount of these flame retardants added greatly affects the foam structure, resulting in a decrease in its overall performance. Grafting flame retardant groups into silicone foam through chemical reactions to achieve intrinsic flame retardancy is also an effective flame retardant modification method, such as phenyl silicone foam, but this method has limited effect on the one hand, and the preparation method is complicated and costly on the other hand.
[0005] Therefore, it is necessary to develop a flame-retardant silicone elastic foam. The prepared foam has both elasticity and flame retardancy without the need to add additional flame retardants and fillers, so that it can have broad application prospects in aerospace, high-speed rail seats, plugging, sealing, filling and other fields. Summary of the invention
[0006] In order to solve the technical problems existing in the prior art, the present invention provides an intrinsic flame-retardant organic silicon elastic foam and a preparation method and application thereof.
[0007] The side active groups of the side active polysiloxane A2 of the present invention react with the hydrogen-containing polysiloxane Si-H to generate gas, which becomes the gas source for foaming; the terminal active polysiloxane A1 reacts with the hydrogen-containing polysiloxane Si-H to form other forms of cross-linking bonds between the main chains, thereby making the cross-linking network flexible and retaining the elasticity of the foam.
[0008] Using side-active polysiloxane A2 alone will result in too high a crosslinking density, and the obtained foam will be a hard foam without elasticity; terminal-active polysiloxane A1 is a long-chain terminal-active polysiloxane, which can reduce the crosslinking density of the foam and make the foam elastic. At the same time, the side-group aromatic ring of A1 can also improve the flame retardant properties of the foam. By controlling the usage ratio of terminal-active polysiloxane A1 and side-active polysiloxane A2, crosslinking can be achieved while foaming, and more silicon-oxygen-silicon structures are generated in the structure, thereby improving the flame retardant properties while retaining the elasticity of the foam.
[0009] One of the objects of the present invention is to provide an intrinsically flame retardant organosilicon elastic foam.
[0010] The intrinsic flame retardant elastic silicone elastic foam is prepared from components including component A and component B;
[0011] The component A comprises terminal active polysiloxane A1, side active polysiloxane A2 and a catalyst; the component B comprises hydrogen-containing polysiloxane.
[0012] In a preferred embodiment of the present invention,
[0013] Based on 100 parts by weight of the terminal active polysiloxane A1, the intrinsic flame retardant organosilicon elastic foam comprises:
[0014]
[0015] In a preferred embodiment of the present invention,
[0016] The structure of the terminal active polysiloxane A1 is:
[0017]
[0018] R1 is hydrogen, hydroxy, alkoxy, epoxy, vinyl, allyl or ketoximate;
[0019] R2 is at least one of ethyl, isopropyl, butyl, octyl, vinyl, and allyl; repeated R2 may be the same or different;
[0020] R3 is at least one of phenyl, benzyl, and naphthyl; repeated R3 may be the same or different;
[0021] 1≤x+y+z≤1000, preferably 100≤x+y+z≤1000;
[0022] x / (x+y+z)=0-1, preferably 0.5-1;
[0023] y / (x+y+z)=0~1;
[0024] z / (x+y+z)=0-1, preferably 0-0.5;
[0025] More preferably,
[0026] The number average molecular weight of the terminal active polysiloxane A1 is 5000 to 100000 g / mol, more preferably 10000 to 80000 g / mol.
[0027] In a preferred embodiment of the present invention,
[0028] The molar percentage of the R3 group of the terminal active polysiloxane A1 to all the side groups of the terminal active polysiloxane A1 is 0-50%, preferably 20-40%; R3 is an aromatic group, which can improve the flame retardant properties of the foam.
[0029] In a preferred embodiment of the present invention,
[0030] The structure of the side-active polysiloxane A2 is:
[0031]
[0032] R4 is at least one of methyl, ethyl, isopropyl, butyl, octyl and phenyl;
[0033] R5 is at least one of methoxy, ethoxy, isopropoxy, butoxy, and tert-butoxy; repeated R5 may be the same or different;
[0034] 1≤m≤2000, preferably 50≤m≤500; 0≤n≤200, preferably 0≤n≤100;
[0035] More preferably,
[0036] The content of R5 groups in the side-active polysiloxane A2 is 0.1 to 1.1 mol / 100 g, preferably 0.5 to 1.1 mol / 100 g.
[0037] In a preferred embodiment of the present invention,
[0038] The structure of the hydrogen-containing polysiloxane in the B component is:
[0039]
[0040] R6 and R7 are independently selected from one of hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, benzyl and naphthyl; and at least one of R6 and R7 is hydrogen, that is, the hydrogen-containing polysiloxane contains hydrogen at the terminal group or the side group, or both the terminal group and the side group contain hydrogen;
[0041] R8 is at least one of methyl, ethyl, isopropyl, butyl, phenyl, benzyl, and naphthyl; repeated R8 may be the same or different;
[0042] 10≤p≤1000, preferably 50≤p≤500;
[0043] 0≤q≤1000, preferably 0≤q≤200;
[0044] More preferably,
[0045] The hydrogen content of the hydrogen-containing polysiloxane in the B component is 0.1 to 1.55 mol / 100 g; the hydrogen content refers to the molar number of active hydrogen in 100 g of the hydrogen-containing polysiloxane.
[0046] In a preferred embodiment of the present invention,
[0047] The catalyst is at least two of chloroplatinic acid, a platinum-containing complex, an organic acid, an organic base, a boron-containing compound, an organic tin, and an organic guanidine; preferably chloroplatinic acid, tetramethylammonium hydroxide, benzyltrimethylammonium hydroxide, platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane complex, tetramethylguanidine, dibutyltin dilaurate, boron trifluoride, di(pentafluorophenyl)borane, tri(pentafluorophenyl)borane, triethylborane, pentamethylcyclopentadienylsilicon cation (Me5CpSi + ) at least two of the following.
[0048] In a preferred embodiment of the present invention,
[0049] The molar amount of the active functional groups of the hydrogen-containing polysiloxane in the B component is greater than the sum of the molar amounts of the active functional groups in A1 and A2 in the A component.
[0050] The second object of the present invention is to provide a method for preparing an intrinsic flame retardant silicone elastic foam, characterized in that the method comprises:
[0051] Firstly, component A and component B are mixed according to the amount of each component, and then component A and component B are mixed to obtain the intrinsic flame retardant and heat insulating elastic silicone foam;
[0052] Preferably, the foaming temperature is 30 to 70° C.; and / or the foaming time is 0.5 to 30 min, preferably 1 to 10 min.
[0053] It can foam at room temperature, and foaming is better between 30 and 70°C. The higher the temperature, the faster the foaming speed. The foaming time can be adjusted by controlling the foaming temperature and the concentration of the catalyst according to the actual application.
[0054] The mixed material can be filled into the desired space and foamed at room temperature; or placed in a mold and placed in a 30-70°C oven for foaming.
[0055] After foaming, curing is performed. Preferably, the curing temperature is 100 to 140° C. and the curing time is 20 to 60 minutes.
[0056] The third object of the present invention is to provide an intrinsic flame retardant silicone elastic foam for use in the fields of aviation, aerospace and electronics.
[0057] Compared with the prior art, the present invention has the following beneficial effects:
[0058] The prior art silicone foam is prepared from hydrogenated polysiloxane, vinyl polysiloxane and terminal hydroxyl polysiloxane with a high binding energy Si-O-Si skeleton, wherein the hydrogenated polysiloxane containing Si-H undergoes a silylation reaction with vinyl to produce crosslinks between chains, and at the same time, the Si-OH of the terminal hydroxyl polysiloxane undergoes a dehydrogenation condensation reaction with Si-H to produce hydrogen, thereby achieving internal crosslinking and foaming to prepare silicone foam. The foam itself has the characteristics of low density, high chemical resistance, a wide operating temperature range, flexibility and heat insulation, which makes it widely used in building materials, transportation and electrical applications. However, the side chain organic groups of the linear polydimethylsiloxane (PDMS) chain are easily ignited when exposed to high temperature environments or flame attacks, which seriously limits its application.
[0059] The intrinsic flame retardant organic silicone elastic foam of the present invention has more aromatic rings and more silicon-oxygen-silicon structures, does not need to add flame retardants, retains the elasticity of the foam while having good flame retardant properties, has the advantages of fast, light, halogen-free, environmentally friendly, non-flammable, etc. It has broad application prospects in closed environments such as aviation, aerospace and high-speed rail carriages.
[0060] The system of the present invention is energy-saving and environmentally friendly, the raw materials are cheap and easily available, no organic solvent needs to be added, the preparation process is simple and convenient, and no complicated equipment and strict experimental conditions are required. DETAILED DESCRIPTION
[0061] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0062] The raw materials used in the examples are all conventional commercially available raw materials;
[0063] Sources of some main raw materials:
[0064] Vinyl-terminated silicone oil: Shandong Dayi Chemical Co., Ltd., DY-V401, number average molecular weight is about 50000 g / mol;
[0065] Methylphenyl-terminated vinyl silicone oil with 40% phenyl content: Guangdong Houxin High-tech Materials Co., Ltd., AM-3050;
[0066] Methyl hydrogen silicone oil with a hydrogen content of 1.55 mol / 100 g: Shin-Etsu Chemical Co., Ltd., KF-99;
[0067] Phenyl hydrogenated silicone oil with a hydrogen content of 0.25 mol / 100 g: Shenzhen Kejunchi Technology Co., Ltd., G616;
[0068] Terminal hydroxymethylphenyl silicone oil: Guangdong Wengjiang Chemical Reagent Co., Ltd., CAS: 63148-59-4;
[0069] Epoxy-terminated methylphenyl silicone oil: Anhui IOTA Silicone Oil Co., Ltd., IOTA105;
[0070] Phenyl hydrogenated silicone oil with a hydrogen content of 0.1 mol / 100 g: Shenzhen Kejunchi Technology Co., Ltd., HD60
[0071] Methylphenyl-terminated vinyl silicone oil with 30% phenyl content: Guangdong Houxin High-tech Materials Co., Ltd., AM-3015;
[0072] Methyl hydrogen silicone oil with a hydrogen content of 1.0 mol / 100 g: Shin-Etsu Chemical Co., Ltd., KF-99;
[0073] Methyl ethyl phenyl vinyl silicone oil: homemade;
[0074] Di(pentafluorophenyl)borane: Shanghai MacLean Biochemical Technology Co., Ltd., CAS: 165612-94-2 Tri(pentafluorophenyl)borane: Shanghai MacLean Biochemical Technology Co., Ltd., CAS: 1109-15-5;
[0075] Tetramethylammonium hydroxide: Shanghai MacLean Biochemical Technology Co., Ltd., CAS: 75-59-2;
[0076] Triethylborane: Shanghai MacLean Biochemical Technology Co., Ltd., CAS: 97-94-9;
[0077] Tetramethylguanidine: Shanghai MacLean Biochemical Technology Co., Ltd., CAS: 80-70-6.
[0078] Methylmethoxy silicone oil with a methoxy content of 1.07 mol / 100 g, methylmethoxy silicone oil with a methoxy content of 0.5 mol / 100 g, ethoxy silicone oil with an ethoxy content of 0.5 mol / 100 g, and methylmethoxy silicone oil with a methoxy content of 1.1 mol / 100 g are all homemade, and the preparation method refers to Chinese invention patent CN101153076A (the invention name is "a polysiloxane resin containing alkoxy groups in the side groups, and its preparation method and use");
[0079] The specific synthesis method of methyl methoxy silicone oil is as follows: weigh 10g of methyl hydrogenated silicone oil with a hydrogen content of 1.6% and 10g of anhydrous methanol in a three-necked flask, stir at 50°C for 30min, slowly drop 0.1g of 10% tetramethylammonium hydroxide methanol solution, react for 6h, add 0.1g of NKC-9 acidic ion exchange resin rinsed three times with methanol to the three-necked flask, pour the reaction solution into a pear-shaped bottle, and rotary evaporate at 55°C for 30min to obtain methyl methoxy silicone oil. Different methoxy contents can be achieved by changing the hydrogen content of the raw material methyl hydrogenated silicone oil.
[0080] The synthesis method of methylethoxy silicone oil is the same as that of methylmethoxy silicone oil, except that anhydrous methanol is replaced by anhydrous ethanol. Different ethoxy contents can be achieved by changing the hydrogen content of the raw material methyl hydrogen silicone oil.
[0081] Methyl ethyl phenyl vinyl silicone oil: homemade;
[0082] The specific synthesis steps of methyl ethyl phenyl vinyl silicone oil are as follows: octamethyl cyclotetrasiloxane, octaethyl cyclotetrasiloxane and octaphenyl cyclotetrasiloxane are added into a three-necked flask at a molar ratio of 8:2:1, and the water is removed at 60°C under a vacuum degree of -0.09 MPa for 1 hour, 0.5 wt% of tetramethyl ammonium hydroxide is added, and the temperature is raised to 110°C. After observing that the viscosity of the system increases, tetramethyl divinyl siloxane (with a molar ratio of 0.1:1 to octaphenyl cyclotetrasiloxane) is added, and the reaction is carried out at 110°C for 8 hours, and then the temperature is raised to 150°C for 30 minutes to remove the catalyst to obtain the product terminal vinyl methyl ethyl phenyl polysiloxane.
[0083] Test method:
[0084] Density: The test standard is GB / T6343-2009.
[0085] Porosity: Calculation is performed according to the following formula: Where Ψ is the porosity, ρ f is the apparent density of the foam, ρ s is the density of solid rubber.
[0086] LOI(%): The test standard is GB / T2406.2-2009.
[0087] UL-94: The test standard is GB / T 8333-2022.
[0088] Thermal conductivity: The thermal conductivity of the silicone foam is tested using a thermal conductivity meter. The sample size is 3mm×4.5mm, the thickness is not limited, and the contact surface with the test electrode is flat.
[0089] Compression strength: The test standard is GB / T 18942.2-2003.
[0090] The parts described in the examples are all parts by weight.
[0091] Example 1
[0092] An intrinsic flame retardant silicone foam comprises a component A and a component B, wherein the component A mainly comprises the following components in parts by weight:
[0093] 100 parts of terminal vinyl silicone oil (number average molecular weight is about 50000g / mol, R3 group content is 0%), 1.5 parts of methylmethoxy silicone oil with a methoxy content of 1.07mol / 100g (polymerization degree is about 100), 0.2 parts of chloroplatinic acid, and 0.05 parts of tris(pentafluorophenyl)borane; component B mainly contains the following components in parts by weight: 25 parts of methyl hydrogen silicone oil with a hydrogen content of 1.55mol / 100g (polymerization degree is about 50).
[0094] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0095] (1) Preparation of component A: According to the formula, vinyl-terminated silicone oil, methylmethoxy silicone oil, chloroplatinic acid and tris(pentafluorophenyl)borane were weighed and mixed thoroughly.
[0096] (2) Preparation of component B: Weigh methyl hydrogen silicone oil according to the formula.
[0097] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 60°C for 1 minute, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0098] Example 2
[0099] An intrinsic flame-retardant organic silicon foam comprises an A component and a B component, wherein the A component mainly comprises the following components in parts by weight: 100 parts of methylphenyl-terminated vinyl silicone oil (number average molecular weight is about 30000 g / mol) in which the molar percentage of phenyl groups in all side groups is 40%, 10 parts of methylmethoxy silicone oil (polymerization degree is about 500) in which the methoxy content is 0.5 mol / 100 g, 0.6 parts of platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane complex, and 0.05 parts of di(pentafluorophenyl)borane; and the B component mainly comprises the following components in parts by weight: 25 parts of phenyl hydrogenated silicone oil (p is about 50, q is about 10) in which the hydrogen content is 0.25 mol / 100 g.
[0100] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0101] (1) Preparation of component A: According to the formula, weigh methylphenyl vinyl-terminated silicone oil, methylmethoxy silicone oil, Custer catalyst, and di(pentafluorophenyl)borane, and mix them thoroughly.
[0102] (2) Preparation of component B: Weigh methyl hydrogen silicone oil according to the formula.
[0103] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 60°C for 1 minute, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0104] Example 3
[0105] An intrinsic flame-retardant organic silicon foam comprises an A component and a B component, wherein the A component mainly comprises the following components in parts by weight: 100 parts of terminal hydroxymethylphenyl silicone oil (number average molecular weight is about 50000 g / mol) in which the molar percentage content of phenyl groups in all side groups is 30%, 0.5 parts of methylmethoxy silicone oil (same as in Example 1) in which the methoxy content is 1.07 mol / 100 g, 0.5 parts of tetramethylammonium hydroxide, and 0.5 parts of triethylborane; and the B component mainly comprises the following components in parts by weight: 50 parts of methylhydrogen silicone oil (same as in Example 1) in which the hydrogen content is 1.55 mol / 100 g.
[0106] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0107] (1) Preparation of component A: Weigh terminal hydroxymethylphenyl silicone oil, methylmethoxy silicone oil, tetramethylammonium hydroxide and triethylborane according to the formula and mix them thoroughly.
[0108] (2) Preparation of component B: Weigh methyl hydrogen silicone oil according to the formula.
[0109] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 60°C for 1 minute, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0110] Example 4
[0111] An intrinsic flame-retardant organic silicon foam comprises a component A and a component B, wherein the component A mainly comprises the following components in parts by weight: 100 parts of epoxy-terminated methylphenyl silicone oil (the difference between the structure and the vinyl-terminated methylphenyl silicone oil in Example 1 is that the terminal group is an epoxy group, and the number average molecular weight is about 70000 g / mol), 10 parts of ethoxy silicone oil with an ethoxy content of 0.5 mol / 100 g (m is about 250, n is about 300), 0.5 parts of tetramethylguanidine catalyst, and 0.05 parts of boron trifluoride; and the component B mainly comprises the following components in parts by weight: 50 parts of phenyl hydrogenated silicone oil with a hydrogen content of 0.1 mol / 100 g (the structural formula is the same as that in Example 2, p is about 200, and q is about 50).
[0112] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0113] (1) Preparation of component A: According to the formula, weigh the epoxy-terminated methyl phenyl silicone oil, ethoxy silicone oil, tetramethylguanidine catalyst, and boron trifluoride, and mix them thoroughly.
[0114] (2) Preparation of component B: Weigh phenyl hydrogen silicone oil according to the formula.
[0115] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 60°C for 1 minute, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0116] Example 5
[0117] An intrinsic flame-retardant organic silicon foam comprises an A component and a B component, wherein the A component mainly comprises the following components in parts by weight: 100 parts of methylphenyl-terminated vinyl silicone oil (having the same structural formula as in Example 2 and a number average molecular weight of about 40,000 g / mol) in which the molar percentage of phenyl groups in all side groups is 30%, 0.5 parts of methylmethoxy silicone oil (having the same structural formula as in Example 1, with m being about 200 and n being 0) having a methoxy content of 1.1 mol / 100 g, 0.5 parts of dibutyltin dilaurate and 0.5 parts of triethylborane; and the B component mainly comprises the following components in parts by weight: 50 parts of methylhydrogen silicone oil (having the same structural formula as in Example 1, with p being about 500 and q being about 200) having a hydrogen content of 1.0 mol / 100 g.
[0118] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0119] (1) Preparation of component A: According to the formula, weigh methylphenyl vinyl-terminated silicone oil, methylmethoxy silicone oil, dibutyltin dilaurate, and triethylborane, and mix them thoroughly.
[0120] (2) Preparation of component B: Weigh methyl hydrogen silicone oil according to the formula.
[0121] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 60°C for 1 minute, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0122] Example 6
[0123] An intrinsic flame-retardant organic silicon foam comprises an A component and a B component, wherein the A component mainly comprises the following components in parts by weight: 100 parts of methylethylphenylvinyl silicone oil (x is about 200, y is about 50, and z is about 30) with a number average molecular weight of about 30000 g / mol and a phenyl group content of 30% in total side groups, 0.5 parts of methylmethoxy silicone oil (same as in Example 1) with a methoxy group content of 1.07 mol / 100 g, 0.3 parts of platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex, and 0.3 parts of boron trifluoride; and the B component mainly comprises the following components in parts by weight: 50 parts of methylhydrogen silicone oil (same as in Example 1) with a hydrogen content of 1.55 mol / 100 g.
[0124] The method for preparing the intrinsic flame retardant elastic silicone foam comprises the following steps:
[0125] (1) Preparation of component A: According to the formula, weigh methylphenyl vinyl-terminated silicone oil, methylmethoxy silicone oil, platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane complex, and boron trifluoride, and mix them thoroughly.
[0126] (2) Preparation of component B: Weigh methyl hydrogen silicone oil according to the formula.
[0127] (3) Component A and component B are mixed evenly and placed in a mold, foamed at 30°C for 10 minutes, and then cured at 120°C for 30 minutes. Intrinsic flame retardant elastic silicone foam is obtained. The performance test results are shown in Table 1.
[0128] Comparative Example 1
[0129] References: Zhang Xianzhen. Preparation and performance research of flame retardant silicone foam materials[D]. Hunan University of Technology, 2021.
[0130] 100 parts of α,ω-dihydroxy polysiloxane (number average molecular weight of about 50,000 g / mol), 20 parts of terminal vinyl silicone oil (number average molecular weight of about 50,000 g / mol), and 0.3 parts of platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex were fully stirred and mixed under a strong electric stirrer for 15 minutes. 20 parts of methyl hydrogen silicone oil with a hydrogen content of 1.55% were added to the stirred base glue, and the mixture was quickly stirred under a strong electric stirrer for 2 minutes and then poured into the mold. After reacting at 30°C for 15 minutes, the mold was placed in a 120°C vacuum drying oven for 3 hours for two-stage treatment. After the reaction was completed, an organic silicone foam material was obtained. The performance test results are shown in Table 1.
[0131] Table 1 Performance test results of foam materials prepared in Examples 1 to 6 and Comparative Example 1
[0132]
[0133] The silicone foam of Comparative Example 1 is prepared from hydrogen-containing polysiloxane, vinyl polysiloxane and terminal hydroxyl polysiloxane having a Si-O-Si skeleton with high binding energy, wherein the hydrogen-containing polysiloxane containing Si-H undergoes a silylation reaction with the vinyl group to produce crosslinks between the chains, and at the same time, the Si-OH of the terminal hydroxyl polysiloxane undergoes a dehydrogenation condensation reaction with the Si-H to produce hydrogen, thereby achieving internal crosslinking and foaming to prepare the silicone foam.
[0134] As shown in Table 1, the LOI of Comparative Example 1 is lower, the vertical combustion level is lower, and the thermal conductivity is higher than that of Examples 1 to 6. This is because the side chain organic groups of the linear polydimethylsiloxane (PDMS) chain of the foam are easily ignited when exposed to high temperature environment or flame attack, which seriously limits its application.
[0135] The intrinsic flame retardant organosilicon elastic foam prepared in Examples 1 to 6 utilizes the side active groups of the side active polysiloxane to react with the hydrogen-containing polysiloxane Si-H to generate gas, which becomes the gas source for foaming; the terminal active polysiloxane reacts with the hydrogen-containing polysiloxane Si-H to form other forms of cross-linking bonds between the main chains, thereby making the cross-linking network flexible and retaining the elasticity of the foam. The intrinsic flame retardant organosilicon elastic foam has more aromatic rings and more silicon-oxygen-silicon structures, does not require the addition of flame retardants, retains the elasticity of the foam while having good flame retardant properties, has the advantages of fast, light weight, halogen-free, environmentally friendly, and non-flammable, and has broad application prospects in closed environments such as aviation, aerospace, and high-speed rail carriages.
Claims
1. An intrinsic flame retardant silicone elastic foam, characterized in that: The intrinsic flame retardant elastic silicone elastic foam is prepared from components including component A and component B; The component A comprises terminal active polysiloxane A1, side active polysiloxane A2 and a catalyst; the component B comprises hydrogen-containing polysiloxane.
2. The intrinsic flame retardant silicone elastic foam according to claim 1, characterized in that: Based on 100 parts by weight of the terminal active polysiloxane A1, the intrinsic flame retardant organosilicon elastic foam comprises:
3. The intrinsic flame retardant silicone elastic foam according to claim 1, characterized in that: The structure of the terminal active polysiloxane A1 is: R1 is hydrogen, hydroxy, alkoxy, epoxy, vinyl, allyl or ketoximate; R2 is at least one of ethyl, isopropyl, butyl, octyl, vinyl, and allyl; repeated R2 may be the same or different; R3 is at least one of phenyl, benzyl, and naphthyl; repeated R3 may be the same or different; 1≤x+y+z≤1000, preferably 100≤x+y+z≤1000; x / (x+y+z)=0-1, preferably 0.5-1; y / (x+y+z)=0~1; z / (x+y+z)=0-1, preferably 0-0.5; x, y, and z cannot be 0 at the same time. It is preferred that x is not 0 or both x and z are not 0. More preferably, The number average molecular weight of the terminal active polysiloxane A1 is 5000 to 100000 g / mol, more preferably 10000 to 80000 g / mol.
4. The intrinsic flame retardant organic silicon elastic foam according to claim 3, characterized in that: The molar percentage of the R3 group of the terminal active polysiloxane A1 to all the side groups of the terminal active polysiloxane A1 is 0 to 50%, preferably 20 to 40%.
5. The intrinsic flame retardant organic silicon elastic foam according to claim 1, characterized in that: The structure of the side-active polysiloxane A2 is: R4 is at least one of methyl, ethyl, isopropyl, butyl, octyl and phenyl; R5 is at least one of methoxy, ethoxy, isopropoxy, butoxy, and tert-butoxy; repeated R5 may be the same or different; 1≤m≤2000, preferably 50≤m≤500; 0≤n≤200, preferably 0≤n≤100; More preferably, The content of R5 groups in the side-active polysiloxane A2 is 0.1 to 1.1 mol / 100 g, preferably 0.5 to 1.1 mol / 100 g.
6. The intrinsic flame retardant organic silicon elastic foam according to claim 1, characterized in that: The structure of the hydrogen-containing polysiloxane in the B component is: R6 and R7 are independently selected from one or more of hydrogen, methyl, ethyl, isopropyl, butyl, phenyl, benzyl, and naphthyl; and at least one of R6 and R7 is hydrogen; R8 is at least one of methyl, ethyl, isopropyl, butyl, phenyl, benzyl, and naphthyl; repeated R8 may be the same or different; 10≤p≤1000, preferably 50≤p≤500; 0≤q≤1000, preferably 0≤q≤200; More preferably, The hydrogen content of the hydrogen-containing polysiloxane in the B component is 0.1 to 1.55 mol / 100 g.
7. The intrinsic flame retardant silicone elastic foam according to claim 1, characterized in that: The catalyst is at least two of chloroplatinic acid, a platinum-containing complex, an organic acid, an organic base, a boron-containing compound, an organic tin, and an organic guanidine; preferably at least two of chloroplatinic acid, tetramethylammonium hydroxide, benzyltrimethylammonium hydroxide, platinum (0)-1,3-diethene-1,1,3,3-tetramethyldisiloxane complex, tetramethylguanidine, dibutyltin dilaurate, boron trifluoride, di(pentafluorophenyl)borane, tri(pentafluorophenyl)borane, triethylborane, and pentamethylcyclopentadienylsilicon cation.
8. The intrinsic flame retardant organic silicon elastic foam according to claim 1, characterized in that: The molar amount of the active functional groups of the hydrogen-containing polysiloxane in the B component is greater than the sum of the molar amounts of the active functional groups in A1 and A2 in the A component.
9. A method for preparing an intrinsic flame retardant silicone elastic foam as claimed in any one of claims 1 to 8, characterized in that The method comprises: Firstly, component A and component B are mixed according to the amount of each component, and then component A and component B are mixed to obtain the intrinsic flame retardant and heat insulating elastic silicone foam; Preferably, the foaming temperature is 30 to 70° C.; and / or the foaming time is 0.5 to 30 min, preferably 1 to 10 min.
10. Use of the intrinsic flame retardant organic silicon elastic foam according to any one of claims 1 to 8 or the intrinsic flame retardant organic silicon elastic foam obtained by the preparation method according to claim 9 in the fields of aviation, aerospace and electronics.
Citation Information
Patent Citations
Flame-retardant organic silicon foam material and preparation method thereof
CN109438992A
Intrinsic flame-retardant and heat-insulating organic silicon polystyrene foam and preparation method thereof
CN113025266A
Foamable silicone composition
US20230287193A1
Method for producing silicone foams
US6359026B1
Cited By
An integrated rigid silicone foam material, and a method of making and use thereof
CN123026920A