Preparation process of high-performance tin-phosphor bronze strip

By adopting multi-step annealing and stress relief treatment in the tin-phosphorus bronze strip preparation process, the problems of poor resilience and insufficient fatigue strength during the contact forming process are solved, and the mechanical properties and stability of the tin-phosphorus bronze strip are improved. , ensuring its reliability and long life in electronic components.

CN118756076APending Publication Date: 2024-10-11JIANGXI YUNTAI COPPER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410828155.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-25
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

In the existing tin-phosphorus bronze preparation process, contacts are prone to orange peel or cracking during the stamping and forming process, and have poor resilience after forming, resulting in unstable electrical connections, and insufficient fatigue strength and stress relaxation resistance, affecting their service life.

Method used

High-performance tin-phosphorus bronze strip preparation process is adopted, including smelting, horizontal continuous casting, heat preservation, pre-rolling, homogenization annealing, cold rolling blanking, recrystallization annealing, degreasing pickling, finish rolling, stress relief annealing and finished product rolling , and perform tension-bending straightening and shearing slitting, and reduce internal residual stress through two recrystallization anneals and stress relief annealing, improving mechanical properties and shape stability.

Benefits of technology

The yield strength, elastic modulus and stress relaxation resistance of the tin-phosphor bronze strip are significantly improved, and its plasticity, ductility and elasticity are enhanced, ensuring the reliability and service life of the contacts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of copper alloys, and provides a high-performance tin-phosphor bronze strip preparation process which comprises the following steps: firstly, sequentially preparing raw materials, sequentially performing smelting and horizontal continuous casting on the prepared raw materials, performing heat preservation treatment after continuous casting, and performing pre-rolling after heat preservation is completed, homogenizing annealing is carried out after pre-rolling is completed; carrying out a heat preservation process on the raw materials after homogenizing annealing, and starting milling and cold rolling cogging after heat preservation is completed. Through two times of recrystallization annealing, stress relief annealing and counterfoil annealing processes, the internal residual stress in the tin-phosphor bronze strip is greatly reduced, so that the mechanical property and the shape stability of the tin-phosphor bronze strip are improved, fine grains and dislocation formed by deformation or hot working are rearranged, and when a new large-grain structure is formed, the mechanical property of the tin-phosphor bronze strip is improved. The grain structure is more uniform and isotropic than previous grains, and the plasticity, ductility and elasticity of the tin-phosphor bronze strip are greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of copper alloys, in particular to a preparation process of a high-performance tin-phosphor bronze strip. Background Art

[0002] After solid solution treatment, combined deformation treatment and low-temperature heat treatment, tin-phosphor bronze has high hardness and strength, and is currently a widely used elastic copper alloy material. With the rapid development of industries such as 5G communications, consumer electronics, and new energy vehicles, electronic products and electronic components are gradually developing in the direction of miniaturization and high integration.

[0003] In this regard, in the existing tin-phosphor bronze preparation process, for connectors with complex structures, there are two major problems with their core components "contact parts": on the one hand, orange peel or even cracking is prone to occur during the stamping process; on the other hand, the contact parts are not resilient enough after molding, the clamping effect is not ideal, and reliable electrical connection cannot be guaranteed.

[0004] Therefore, in order to better enable the connector to complete the electrical connection function, the copper alloy strip is not only required to have good bending performance, that is, 90° bending bad direction R / t≤1.5, so as to ensure that the stamping does not crack, but also must ensure that the connector has excellent resilience after forming. Therefore, the high-demand bronze alloy for connectors is required to have a yield strength greater than 650MPa and an elastic modulus greater than 115GPa. In addition, fatigue strength and stress relaxation resistance are related to the service life and stability of the contact, because the contact not only has a certain amount of elastic deformation during use, but also needs to carry a certain current load at the same time, so a preparation process for producing high-performance tin-phosphor bronze strip is required. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a high-performance tin-phosphorus bronze strip preparation process, which solves the problem that the tin-phosphorus bronze strip lacks excellent high performance in terms of comprehensive properties such as yield strength, elastic modulus and stress relaxation resistance.

[0006] To achieve the above objectives, the present invention is implemented by the following technical solutions: A high-performance tin-phosphor bronze strip preparation process comprises the following steps:

[0007] Step 1: First, the raw materials are prepared in sequence, and the prepared raw materials are melted and horizontally continuously cast in sequence, and after the continuous casting is completed, they are heat-insulated, and after the heat-insulation is completed, they are pre-rolled, and after the pre-rolling is completed, they are homogenized and annealed;

[0008] Step 2, after the homogenization annealing in step 1, the raw material is subjected to a heat preservation process, and after the heat preservation is completed, the milling surface is started and the cold rolling is performed, and after the completion, the first recrystallization annealing is performed, and after the first recrystallization annealing is completed, the first degreasing pickling is performed, and after the pickling is completed, the raw material is dried, and after the completion, the intermediate rolling is performed;

[0009] Step 3, after the raw material has completed the intermediate rolling, the raw material is subjected to a second recrystallization annealing, and the raw material is subjected to a second degreasing pickling and drying. After the surface of the raw material is dried, the finish rolling is started, and after the finish rolling is completed, the stress relief annealing is performed, and after the bottom annealing is completed, the raw material is finally rolled into a finished product;

[0010] Step 4: After rolling, the finished product is milled, bent, straightened, and cut into strips.

[0011] Preferably, in the step 1, the holding temperature after continuous casting is 300-550° C., and the holding time is 3-5 hours.

[0012] Preferably, the processing rate of the pre-rolling in the step 1 is controlled at 25% to 45%, and the deformation amount of the cold-rolling blanking is 75% to 85%.

[0013] Preferably, in step 2, the homogenization annealing temperature is 650-880° C., and the holding time is 7-12 hours.

[0014] Preferably, the temperature of the first recrystallization annealing in step 2 is 510-570° C., and the holding time is 2-4 hours.

[0015] Preferably, the processing rate of the intermediate rolling in the step 2 is controlled at 40-65%.

[0016] Preferably, the second recrystallization annealing temperature in step three is 480-550° C., and the holding time is 3-4 hours.

[0017] Preferably, the processing rate of the finishing rolling in the step three is controlled at 40-55%, and the processing rate of the finished product rolling is controlled at 30-55%.

[0018] Preferably, in step three, the stress relief annealing temperature is 280-330° C. and the time is 2-4 hours.

[0019] Preferably, in step 4, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower surfaces.

[0020] The present invention provides a high-performance tin-phosphor bronze strip preparation process, which has the following beneficial effects:

[0021] The present invention reduces the internal residual stress in the tin-phosphor bronze strip to a great extent through two recrystallization annealings, as well as stress relief annealing and bottom annealing processes, thereby improving its mechanical properties and shape stability. When the fine grains and dislocations formed by deformation or hot working are rearranged to form a new large grain structure, the grain structure is more uniform and more isotropic than the previous grains, thereby greatly improving the plasticity, ductility and elasticity of the tin-phosphor bronze strip. DETAILED DESCRIPTION

[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0023] The embodiment of the present invention provides a high-performance tin-phosphor bronze strip preparation process, comprising the following steps:

[0024] Step 1, firstly, the raw materials are prepared in sequence, the prepared raw materials are melted and horizontally continuously cast in sequence, and after continuous casting, they are subjected to heat preservation treatment, and after heat preservation, they are pre-rolled, and after pre-rolling, they are subjected to homogenization annealing. In the step 1, the heat preservation temperature after continuous casting is 300-550° C., the heat preservation time is 3-5 hours, the processing rate of pre-rolling is controlled at 25%-45%, and the deformation amount of the cold rolling blank is 75%-85%;

[0025] Step 2, after the homogenization annealing in step 1, the raw material is subjected to a heat preservation process, and after the heat preservation is completed, the milling surface is started and the cold rolling is performed, and after the completion, the first recrystallization annealing is performed, and after the first recrystallization annealing is completed, the first degreasing pickling is performed, and after the pickling is completed, the drying is performed, and after the completion, the intermediate rolling is performed, the homogenization annealing temperature is 650-880°C, the heat preservation time is 7-12h, the temperature of the first recrystallization annealing is 510-570°C, the heat preservation time is 2-4h, and the processing rate of the intermediate rolling is controlled at 40-65%;

[0026] Step 3, after the raw material is subjected to the intermediate rolling in step 2, the raw material is subjected to a second recrystallization annealing, and the raw material is subjected to a second degreasing pickling and drying. After the surface of the raw material is dried, the finishing rolling is started, and after the finishing rolling is completed, the stress relief annealing is performed. After the bottom annealing is completed, the raw material is subjected to the final finished product rolling. The second recrystallization annealing temperature is 480-550°C, the holding time is 3-4h, the finishing rolling processing rate is controlled at 40-55%, the finished product rolling processing rate is controlled at 30-55%, the stress relief annealing temperature is 280-330°C, and the time is 2-4h;

[0027] Step 4: After rolling, the finished product is first milled and then subjected to bending and straightening treatment, and then sheared into strips. In step 4, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower milling surfaces.

[0028] Through two recrystallization annealings, as well as stress relief annealing and bottom annealing processes, the internal residual stress in the tin-phosphorus bronze strip is greatly reduced, thereby improving its mechanical properties and shape stability. In addition, the fine grains and dislocations formed by deformation or hot working are rearranged to form a new large-grain structure. The grain structure is more uniform and isotropic than the previous grains, which greatly improves the plasticity, ductility and elasticity of the tin-phosphorus bronze strip.

[0029] The above scheme is introduced below in conjunction with specific embodiments.

[0030] Embodiment 1:

[0031] A high-performance tin-phosphor bronze strip preparation process comprises the following steps:

[0032] Step 1, firstly, the raw materials are prepared in sequence, and the prepared raw materials are melted and horizontally continuously cast in sequence, and after the continuous casting is completed, they are subjected to heat preservation treatment, and after the heat preservation is completed, they are pre-rolled, and after the pre-rolling is completed, homogenization annealing is performed, wherein the heat preservation temperature after continuous casting in the step 1 is 380° C., the heat preservation time is 5 hours, the processing rate of pre-rolling is controlled at 25% to 45%, and the deformation amount of the cold rolling blank is 75% to 85%;

[0033] Step 2, after the homogenization annealing in step 1, the raw material is subjected to a heat preservation process, and after the heat preservation is completed, the milling surface is started and the cold rolling is performed, and after the completion, the first recrystallization annealing is performed, and after the first recrystallization annealing is completed, the first degreasing pickling is performed, and after the pickling is completed, the drying is performed, and after the completion, the intermediate rolling is performed, the homogenization annealing temperature is 680° C., the heat preservation time is 10 hours, the temperature of the first recrystallization annealing is 520° C., the heat preservation time is 3 hours, and the processing rate of the intermediate rolling is controlled at 40-65%;

[0034] Step 3, after the raw material is subjected to the intermediate rolling in step 2, the raw material is subjected to a second recrystallization annealing, and the raw material is subjected to a second degreasing pickling and drying. After the surface of the raw material is dried, the finishing rolling is started, and after the finishing rolling is completed, the stress relief annealing is performed. After the bottom annealing is completed, the raw material is subjected to the final finished product rolling. The second recrystallization annealing temperature is 500°C, the holding time is 4h, the finishing rolling processing rate is controlled at 40-55%, the finished product rolling processing rate is controlled at 30-55%, the stress relief annealing temperature is 280°C, and the time is 4h;

[0035] Step 4: After rolling, the finished product is first milled and then subjected to bending and straightening treatment, and then sheared into strips. In step 4, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower milling surfaces.

[0036] In this regard, the first embodiment of the present invention reduces various annealing temperatures and prolongs the holding time of various annealing processes, so that the grain structure of the prepared tin-phosphorus bronze strip is more uniform and more isotropic, the performance of the tin-phosphorus bronze strip is improved, and the finished product is more stable and controllable, but its production efficiency is lower.

[0037] Embodiment 2:

[0038] A high-performance tin-phosphor bronze strip preparation process comprises the following steps:

[0039] Step 1, firstly, the raw materials are prepared in sequence, and the prepared raw materials are melted and horizontally continuously cast in sequence, and after the continuous casting is completed, they are subjected to heat preservation treatment, and after the heat preservation is completed, they are pre-rolled, and after the pre-rolling is completed, homogenization annealing is performed, wherein the heat preservation temperature after continuous casting in the step 1 is 540° C., the heat preservation time is 3 hours, the processing rate of pre-rolling is controlled at 25% to 45%, and the deformation amount of the cold rolling blank is 75% to 85%;

[0040] Step 2, after the homogenization annealing in step 1, the raw material is subjected to a heat preservation process, and after the heat preservation is completed, the milling surface is started and the cold rolling is performed, and after the completion, the first recrystallization annealing is performed, and after the first recrystallization annealing is completed, the first degreasing pickling is performed, and after the pickling is completed, the drying is performed, and after the completion, the intermediate rolling is performed, the homogenization annealing temperature is 850° C., the heat preservation time is 9h, the temperature of the first recrystallization annealing is 560° C., the heat preservation time is 2h, and the processing rate of the intermediate rolling is controlled at 40-65%;

[0041] Step 3, after the raw material is subjected to the intermediate rolling in step 2, the raw material is subjected to a second recrystallization annealing, and the raw material is subjected to a second degreasing pickling and drying. After the surface of the raw material is dried, the finishing rolling is started, and after the finishing rolling is completed, the stress relief annealing is performed, and after the bottom annealing is completed, the raw material is subjected to the final finished product rolling, the second recrystallization annealing temperature is 540°C, the holding time is 3h, the finishing rolling processing rate is controlled at 40-55%, the finished product rolling processing rate is controlled at 30-55%, the stress relief annealing temperature is 330°C, and the time is 2h;

[0042] Step 4: After rolling, the finished product is first milled and then subjected to bending and straightening treatment, and then sheared into strips. In step 4, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower milling surfaces.

[0043] In this regard, the second embodiment increases the temperature of various annealing processes, reduces the holding time of various annealing processes, and greatly improves production efficiency. However, the performance of the tin-phosphorus bronze strip prepared thereby cannot reach the optimum, and the quality of the finished product preparation is more controllable and reduced.

[0044] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A process for preparing high-performance tin-phosphor bronze strip, characterized in that: The following steps are involved: Step 1: First, the raw materials are prepared in sequence, and the prepared raw materials are melted and horizontally continuously cast in sequence, and after the continuous casting is completed, they are heat-insulated, and after the heat-insulation is completed, they are pre-rolled, and after the pre-rolling is completed, they are homogenized and annealed; Step 2, after the homogenization annealing in step 1, the raw material is subjected to a heat preservation process, and after the heat preservation is completed, the milling surface is started and the cold rolling is performed, and after the completion, the first recrystallization annealing is performed, and after the first recrystallization annealing is completed, the first degreasing pickling is performed, and after the pickling is completed, the raw material is dried, and after the completion, the intermediate rolling is performed; Step 3: After the intermediate rolling in step 2 is completed, the raw material is subjected to a second recrystallization annealing, and the raw material is subjected to a second degreasing pickling and drying. After the surface of the raw material is dried, the finish rolling is started, and after the finish rolling is completed, the stress relief annealing is performed, and after the bottom annealing is completed, the raw material is finally rolled into a finished product; Step 4: After rolling, the finished product is milled, bent, straightened, and cut into strips.

2. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: In the step 1, the holding temperature after continuous casting is 300-550° C., and the holding time is 3-5 hours.

3. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: The processing rate of the pre-rolling in the step 1 is controlled at 25% to 45%, and the deformation amount of the cold-rolling blank is 75% to 85%.

4. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: In the step 2, the homogenization annealing temperature is 650-880° C., and the holding time is 7-12 hours.

5. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: The temperature of the first recrystallization annealing in step 2 is 510-570° C., and the holding time is 2-4 hours.

6. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: The processing rate of the intermediate rolling in the step 2 is controlled at 40-65%.

7. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: The second recrystallization annealing temperature in step three is 480-550° C., and the holding time is 3-4 hours.

8. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: In the step three, the processing rate of the finishing rolling is controlled at 40-55%, and the processing rate of the finished product rolling is controlled at 30-55%.

9. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: In the step three, the stress relief annealing temperature is 280-330° C. and the time is 2-4 hours.

10. A process for preparing a high performance tin phosphor bronze strip according to claim 1, characterized in that: In the step 4, the milling surface of the raw material is 0.35 to 0.6 mm on the upper and lower surfaces.