Plating solution for electro-deposition of platinum layer on surface of nickel-based superalloy and electro-deposition method
By using a plating solution composed of tetraammine platinum hydrogen phosphate and the like, the problem of poor quality platinum layer on the surface of nickel-based high-temperature alloys is solved, the uniformity and stability of the platinum coating are achieved, and the electrodeposition efficiency and performance are improved.
Patent Information
- Application Number
- CN202411083520.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-11
AI Technical Summary
The quality of the platinum layer on the surface of existing nickel-based high-temperature alloys is poor. The tetravalent platinum in the main salt ammonium hexachloroplatinate is easily converted into divalent platinum, resulting in instability of the plating solution, low current efficiency, and diffusion of chlorine elements in the coating affecting performance.
A plating solution composed of tetraammine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecyl sulfonate and sodium hydroxide is used to improve the dispersion ability and stability of the platinum coating by controlling the concentration and pH value. properties, avoid pinholes and burr defects, and use deionized water as the balance to form a non-toxic and harmless electrolyte.
It improves the thickness distribution uniformity and quality of the platinum coating, enhances the control stability of the electrodeposition process, avoids the diffusion of chlorine elements, and achieves efficient electrodeposition and the preparation of high-performance platinum layers.
Smart Images

Figure CN118756268A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of surface treatment, in particular to a plating solution and an electroplating method for electroplating a platinum layer on the surface of a nickel-based high-temperature alloy. Background Art
[0002] At present, the main salt compounds used in the plating solution for electroplating platinum on nickel-based high-temperature alloys mainly include dinitrosodiammine platinum, hydroxyl complexes, ammonia (amine) complexes and chlorine complexes.
[0003] CN104271811A discloses a plating solution for electroplating platinum, which uses ammonium hexachloroplatinate ((NH4)2PtCl6) as the main salt of the plating solution, diammonium phosphate and ammonium dihydrogen phosphate as buffers, and sodium phosphate and the like as conductive salts; the valence state of platinum in the main salt ammonium hexachloroplatinate of the plating solution is tetravalent platinum, which is an unstable high-valence state. During the electroplating process, tetravalent platinum ions are easily converted into divalent ones, causing the plating solution to be unstable, thereby causing the plating solution to fail; in addition, the main salt in the plating solution contains chloride ions, which will be brought into the coating during the electroplating process, causing the chlorine element in the coating to diffuse through the coating to the substrate under high temperature conditions, thereby seriously affecting the coating and industrial performance and reducing the service life of the workpiece.
[0004] CN108130566A provides a plating solution for electroplating platinum, which uses dinitrosodiammine platinum as the main salt, aminosulfonic acid and sodium citrate as the complexing agent, and sodium nitrite and ammonium nitrate as the conductive salt. The current efficiency of the plating solution is low, only about 20%, and the deposition speed is slow, the plating speed is about 2μm / h, which can no longer meet the needs of electroplating functional platinum layers of nickel-based high-temperature alloys. Therefore, it is of great significance to develop an electrolyte and an electroplating method thereof with simple components, easy maintenance, few decomposition products, easy analysis, high current efficiency, and fast electroplating speed, for electroplating platinum layers and preparing high-performance PtAl coatings. Summary of the invention
[0005] The first aspect of the present invention aims to provide a plating solution for electrodepositing a platinum layer on the surface of a nickel-based high-temperature alloy, so as to solve the technical problem of poor quality of the platinum layer on the surface of the existing nickel-based high-temperature alloy.
[0006] The first aspect of the present invention provides a plating solution for electrodepositing a platinum layer on the surface of a nickel-based high-temperature alloy, which consists of tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecyl sulfate, sodium hydroxide and deionized water. In terms of platinum, the concentration of tetraamine platinum hydrogen phosphate is 2g / L to 10g / L; the concentration of disodium ethylenediaminetetraacetate is 20g / L to 40g / L; the concentration of sodium phosphate is 10g / L to 30g / L; the concentration of sodium dodecyl sulfate is 0.5g / L to 1g / L, the pH of the plating solution is 9.5 to 10.5, and the balance is deionized water.
[0007] The plating solution for electroplating a platinum layer on the surface of a nickel-based high-temperature alloy provided in the first aspect of the present invention has the following beneficial effects:
[0008] The plating solution of the present invention uses tetraammine platinum hydrogen phosphate as a main salt and disodium ethylenediaminetetraacetate as a complexing agent. By controlling the concentrations of the main salt and the complexing agent, the electrolyte has good dispersibility, and the thickness distribution uniformity of the platinum coating is improved. By using an appropriate amount of sodium dodecylsulfonate as a surfactant, defects such as pinholes and burrs in the platinum layer are avoided, and the quality of the platinum layer is improved. In addition, by adding phosphate and hydrogen phosphate as a buffer system, the electrolyte can withstand the instability of the electrodeposition process caused by pH fluctuation or change in the content of plating solution components in a large range, and the control stability of the electrodeposition process is improved. In addition, the electrolyte of the present invention is non-toxic and harmless and does not pollute the environment.
[0009] The second aspect of the present invention aims to provide an electrodeposition method to solve the technical problem of poor quality of the platinum layer on the surface of the nickel-based high-temperature alloy.
[0010] The second aspect of the present invention provides an electrodeposition method, comprising:
[0011] Clean the surface of nickel-based high-temperature alloy;
[0012] The above-mentioned plating solution is used to electro-deposit the surface of the nickel-based high-temperature alloy to prepare a platinum layer on the surface of the nickel-based high-temperature alloy.
[0013] The beneficial effects brought about by the electrodeposition method provided in the second aspect of the present invention are:
[0014] By using the above-mentioned plating solution in the electroplating method, the electroplating method accordingly has all the advantages of the above-mentioned plating solution, which will not be described in detail here.
[0015] In an optional technical solution, the cleaning of the surface of the nickel-based high-temperature alloy includes sequentially performing sandblasting, electrolytic degreasing and water washing.
[0016] In an optional technical solution, the sand used for sandblasting is white corundum sand and / or glass beads; the sandblasting pressure is 0.1MPa to 0.3MPa, the sandblasting angle is 70° to 90°, the sandblasting distance is 90mm to 150mm, and the time is 2min to 6min.
[0017] In an optional technical solution, the degreasing liquid used in the electrolytic degreasing includes sodium hydroxide, sodium phosphate, sodium carbonate and deionized water; 10g / L~20g / L of sodium hydroxide, 20g / L~40g / L of sodium phosphate, and 10g / L~20g / L of sodium carbonate; during the electrolytic degreasing process, the voltage is 2V, the temperature is maintained at room temperature, and the time is 2~5min; cathode degreasing is adopted, and titanium mesh is selected as the anode.
[0018] In the optional technical solution, during the electroplating process, the plating solution temperature is 85°C to 90°C, the pH value is 9.5 to 10.5, and the electroplating current density is 0.5A / dm 2 ~2A / dm 2 , the electrodeposition time is 0.5h to 2h; the pH value is adjusted by sodium hydroxide.
[0019] In an optional technical solution, during the electrodeposition process, tetraammineplatinum hydrogen phosphate solution is added to maintain the concentration of platinum in the plating solution.
[0020] In an optional technical solution, the concentration of the tetraamineplatinum hydrogen phosphate solution is 2 g / L to 10 g / L, calculated as platinum.
[0021] In an optional technical solution, during the electrodeposition process, gas stirring or cathode movement is applied, and during the electrodeposition process, a filter pump is used to circulate and filter the plating solution.
[0022] In an optional technical solution, the platinum layer on the surface of the nickel-based high-temperature alloy is subjected to a dehydrogenation annealing treatment, and the temperature of the dehydrogenation annealing treatment is 200° C. to 400° C., and the time is 2 h to 4 h. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the background technology, the drawings required for use in the embodiments or the background technology description will be briefly introduced below. Obviously, the drawings in the following description are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0024] Figure 1 It is a schematic flow chart of the electrodeposition method provided by the present invention;
[0025] Figure 2 is the XRD spectrum of the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in Example 1 of the present invention;
[0026] Figure 3 is a surface SEM image of the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in Example 1 of the present invention;
[0027] Figure 4 is a cross-sectional SEM image of the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in Example 1 of the present invention;
[0028] Figure 5 is a surface SEM image of the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy obtained in Example 2 of the present invention;
[0029] Figure 6is a cross-sectional SEM image of the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy obtained in Example 2 of the present invention;
[0030] Figure 7 This is a cross-sectional SEM image of the platinum layer on the surface of the DD419 nickel-based high-temperature alloy obtained in Example 3 of the present invention. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more clearly understood, the specific embodiments of the present invention are described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] The plating solution for electroplating a platinum layer on the surface of a nickel-based high-temperature alloy provided by the present invention consists of tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecyl sulfonate, sodium hydroxide and deionized water. In terms of platinum, the concentration of tetraamine platinum hydrogen phosphate is 2 g / L-10 g / L; the concentration of disodium ethylenediaminetetraacetate is 20 g / L-40 g / L; the concentration of sodium phosphate is 10 g / L-30 g / L; the concentration of sodium dodecyl sulfonate is 0.5 g / L-1 g / L, the pH value of the plating solution is 9.5-10.5, and the balance is deionized water.
[0033] The plating solution of the present invention uses tetraammine platinum hydrogen phosphate as a main salt and disodium ethylenediaminetetraacetate as a complexing agent. By controlling the concentrations of the main salt and the complexing agent, the electrolyte has good dispersibility, and the thickness distribution uniformity of the platinum coating is improved. By using an appropriate amount of sodium dodecylsulfonate as a surfactant, defects such as pinholes and burrs in the platinum layer are avoided, and the quality of the platinum layer is improved. In addition, by adding phosphate and hydrogen phosphate as a buffer system, the electrolyte can withstand the instability of the electrodeposition process caused by pH fluctuation or change in the content of plating solution components in a large range, and the control stability of the electrodeposition process is improved. In addition, the electrolyte of the present invention is non-toxic and harmless and does not pollute the environment.
[0034] Moreover, in the present application, platinum is added in combination with ammonia, rather than chloride ions as in CN104271811A. Moreover, during the electrodeposition process, ammonia will not be brought into the deposited platinum layer.
[0035] Among them, those skilled in the art should understand that, although the concentration of sodium hydroxide is not clearly stated in the present application, the pH of the plating solution is 9.5 to 10.5, that is, the hydrogen ion concentration is 10 -10.5 mol / L~10 -9.5mol / L, and there are hydrogen phosphate and phosphate as a buffer system to control the hydrogen ion concentration, and the hydrolysis of sodium dodecyl sulfate and disodium ethylenediaminetetraacetate can also make water release hydroxide ions to control the pH value. Therefore, based on the influence of the above substances on the pH, the concentration and total amount of sodium hydroxide added can be determined by those skilled in the art based on their existing chemical knowledge, and there is no need for specific description in this application.
[0036] Figure 1 Schematic diagram of the process of the electrodeposition method provided by the present invention; Figure 1 As shown, the electrodeposition method provided by the present invention includes: cleaning the surface of the nickel-based high-temperature alloy; using the above-mentioned plating solution to electro-deposit the surface of the nickel-based high-temperature alloy to prepare a platinum layer on the surface of the nickel-based high-temperature alloy.
[0037] The beneficial effects brought by the electrodeposition method provided by the present invention are:
[0038] By using the above-mentioned plating solution in the electroplating method, the electroplating method accordingly has all the advantages of the above-mentioned plating solution, which will not be described in detail here.
[0039] like Figure 1 As shown, optionally, cleaning the surface of the nickel-based high-temperature alloy includes sequentially performing sandblasting, electrolytic degreasing and water washing.
[0040] By sandblasting, dirt such as scale on the surface of the high-temperature alloy can be removed first, then the oil can be removed by electrolytic degreasing, and finally the solute of the electrolytic degreasing can be removed by water washing to improve the cleanliness of the surface of the nickel-based high-temperature alloy, so that the platinum layer can be fully electrodeposited on the surface of the nickel-based high-temperature alloy.
[0041] Optionally, the sand used for sand blasting is white corundum sand and / or glass beads; the pressure of sand blasting is 0.1MPa to 0.3MPa, the sand blasting angle is 70° to 90°, the sand blasting distance is 90mm to 150mm, and the time is 2min to 6min.
[0042] By using the above-mentioned sand particles and selecting the above-mentioned parameters, the oxide scale on the surface of the nickel-based high-temperature alloy can be effectively removed.
[0043] Optionally, the degreasing liquid used for electrolytic degreasing includes sodium hydroxide, sodium phosphate, sodium carbonate and deionized water; 10g / L~20g / L of sodium hydroxide, 20g / L~40g / L of sodium phosphate, 10g / L~20g / L of sodium carbonate; during the electrolytic degreasing process, the voltage is 2V, the temperature is maintained at room temperature, and the time is 2~5min; cathode degreasing is adopted, and titanium mesh is selected as the anode.
[0044] By using the above substances as cleaning agents for electrolytic degreasing and matching the above parameters, oil stains on the surface of nickel-based high-temperature alloys can be effectively removed, and chloride ions will not be introduced into the nickel-based high-temperature alloys, thereby avoiding reducing the service life of the nickel-based high-temperature alloys.
[0045] Optionally, during the electroplating process, the plating solution temperature is 85°C to 90°C, the pH value is 9.5 to 10.5, and the electroplating current density is 0.5A / dm 2 ~2A / dm 2 , electrodeposition time is 0.5h~2h; pH value is adjusted with sodium hydroxide.
[0046] By controlling the process parameters during the electrodeposition process and evenly distributing the electrodeposited anode around the cathode, a coating with uniform thickness distribution and good interface bonding with the nickel-based high-temperature alloy can be prepared. The platinum coating is uniform and dense, without peeling or cracking, thereby ensuring the quality of the PtAl coating on the surface of the nickel-based high-temperature alloy. In addition, a platinum coating with a large thickness (>15μm) is prepared by electrodeposition on the surface of complex-shaped workpieces, expanding the application range of nickel-based high-temperature alloys and platinum coatings.
[0047] Optionally, during the electrodeposition process, tetraammine platinum hydrogen phosphate solution is added to maintain the concentration of platinum in the plating solution.
[0048] The plating solution of the present invention has high stability, and under the premise of ensuring the pH value of the plating solution, by adding the main salt to the plating solution, the plating solution is reused, and the amount of auxiliary salt used is reduced. Moreover, the platinum in the plating solution can be completely recovered after use, which greatly reduces the cost of electrodeposition.
[0049] Optionally, in the tetraamine platinum hydrogen phosphate solution, the concentration of the tetraamine platinum hydrogen phosphate solution is 2 g / L to 10 g / L, calculated as platinum.
[0050] Optionally, during the electrodeposition process, gas stirring or cathode movement is applied, and a filter pump is used to circulate and filter the plating solution during the electrodeposition process.
[0051] During the gas stirring process, gas may be introduced into the plating solution to promote the flow of the plating solution. From the perspective of lower cost, air may be introduced into the plating solution, and of course, a gas with more stable chemical properties such as nitrogen or an inert gas such as argon or helium may also be used.
[0052] like Figure 1 As shown, optionally, the platinum layer on the surface of the nickel-based high-temperature alloy is subjected to a dehydrogenation annealing treatment, and the temperature of the dehydrogenation annealing treatment is 200° C. to 400° C., and the time is 2 h to 4 h.
[0053] The platinum layer on the surface of the nickel-based high-temperature alloy is subjected to a dehydrogenation annealing heat treatment to reduce the hydrogen content in the surface platinum layer and prevent hydrogen embrittlement caused by hydrogen.
[0054] In summary, the electrodeposition method comprises the following steps:
[0055] Sandblasting the nickel-based high-temperature alloy;
[0056] Electrolytically degreasing and water washing the nickel-based high-temperature alloy after sandblasting;
[0057] Electrodepositing a platinum layer on the surface of the washed nickel-based high-temperature alloy;
[0058] The surface platinum layer is subjected to annealing heat treatment to remove hydrogen.
[0059] Embodiment 1:
[0060] The plating solution provided in this embodiment for electrodepositing a platinum layer on the surface of a nickel-based high-temperature alloy is prepared by mixing tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecylbenzene sulfonate and deionized water. The content of each component in the electrolyte is: 5 g / L (in terms of platinum) of tetraamine platinum hydrogen phosphate, 20 g / L of disodium ethylenediaminetetraacetate, 10 g / L of sodium phosphate, 0.5 g / L of sodium dodecylbenzene sulfonate, an appropriate amount of sodium hydroxide to adjust the pH, and the balance is deionized water.
[0061] The electrodeposition method provided in this embodiment comprises the following steps:
[0062] Step 1: The surface of the K403 nickel-based high-temperature alloy is sandblasted and degreased in sequence; the sand used for sandblasting is white corundum, the sand size is 100 mesh, the sandblasting pressure is 0.2MPa, the sandblasting angle is 90°, the sandblasting distance is 100mm, and the sandblasting times are 2 times.
[0063] Step 2: Place the K403 nickel-based high-temperature alloy after sandblasting in the degreasing tank for electrolytic degreasing. The degreasing liquid used is composed of: 10g / L sodium hydroxide, 20g / L sodium phosphate, 20g / L sodium carbonate, and the rest is deionized water. Electrolytic degreasing process parameters: voltage is 2V, temperature is room temperature, and time is 5min. Cathode degreasing is used, and titanium mesh is used as anode. Then rinse with deionized water.
[0064] Step 3: Place the washed K403 nickel-based high-temperature alloy in a solution with a pH of 10, a plating temperature of 90°C, and an electrodeposition current density of 1A / dm 2 Electrodeposition was carried out under the conditions of 2h. During the electrodeposition process, the concentration of platinum in the plating solution was maintained at 5g / L calculated as platinum by adding tetraamine platinum hydrogen phosphate, and a platinum layer on the surface of K403 nickel-based high-temperature alloy was obtained; the pH value was adjusted by sodium hydroxide; the anode used in the electrodeposition process was a platinum-plated titanium mesh, and the cathode was a K403 nickel-based high-temperature alloy workpiece. The anode platinum-titanium mesh was evenly placed around the workpiece, and the distance between the anode and the cathode nickel-based high-temperature alloy was 8cm; a filter pump was used to circulate and filter the plating solution during the electrodeposition process.
[0065] Step 4: subjecting the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in step 3 to dehydrogenation annealing; the temperature of the annealing dehydrogenation treatment is 200° C. and the time is 4 hours.
[0066] Figure 2 is the XRD spectrum of the platinum layer on the surface of K403 nickel-based high-temperature alloy obtained in this embodiment. Figure 2 It can be seen that a single-phase platinum layer is formed on the surface of the K403 nickel-based high-temperature alloy by the electrodeposition method of the present invention.
[0067] Figure 3 is the overall SEM image of the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in this embodiment. Figure 3 It can be seen that the surface condition of the platinum layer on the surface of the K403 nickel-based high-temperature alloy in this embodiment is good, without peeling or cracking.
[0068] Figure 4 is a cross-sectional SEM image of the platinum layer on the surface of the K403 nickel-based high-temperature alloy obtained in this embodiment. Figure 4 It can be seen that the platinum layer on the surface of the K403 nickel-based high-temperature alloy in this embodiment is relatively thick, about 16.5 μm, indicating that the platinum layer prepared by the plating solution has low stress and the interface between the plating layer and the K403 nickel-based high-temperature alloy is well bonded.
[0069] Embodiment 2:
[0070] The plating solution provided in this embodiment for electrodepositing a platinum layer on the surface of a nickel-based high-temperature alloy is prepared by mixing tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecylbenzene sulfonate and deionized water. The content of each component in the electrolyte is: 8 g / L (in terms of platinum) of tetraamine platinum hydrogen phosphate, 25 g / L of disodium ethylenediaminetetraacetate, 20 g / L of sodium phosphate, 0.8 g / L of sodium dodecylbenzene sulfonate, an appropriate amount of sodium hydroxide to adjust the pH, and the balance is deionized water.
[0071] The electrodeposition method provided in this embodiment comprises the following steps:
[0072] Step 1: The surface of the GH4169 nickel-based high-temperature alloy is sandblasted and degreased in sequence; the sand used for sandblasting is white corundum, the sand size is 150 mesh, the sandblasting pressure is 0.2MPa, the sandblasting angle is 80°, the sandblasting distance is 90mm, and the sandblasting times are 3 times.
[0073] Step 2: Place the sandblasted GH4169 nickel-based high-temperature alloy in a degreasing tank for electrolytic degreasing. The degreasing liquid used is composed of 15g / L sodium hydroxide, 30g / L sodium phosphate, 25g / L sodium carbonate, and the rest is deionized water. Electrolytic degreasing process parameters: voltage is 2V, temperature is room temperature, and time is 3min. Cathode degreasing is used, and titanium mesh is used as anode. Then rinse with deionized water.
[0074] Step 3: Place the washed GH4169 nickel-based high-temperature alloy in an electrolyte solution with a pH of 10.5, an electrolyte temperature of 90°C, and an electrodeposition current density of 0.5A / dm 2 The electrodeposition was carried out under the conditions of for 1h. During the electrodeposition process, the concentration of platinum in the plating solution was controlled by adding tetraamine platinum hydrogen phosphate, which was 8g / L calculated as platinum, to obtain a platinum layer on the surface of the GH4169 nickel-based high-temperature alloy. The pH value was adjusted by sodium hydroxide. The anode used in the electrodeposition process was a platinum-titanium mesh, and the cathode was a GH4169 nickel-based high-temperature alloy workpiece. The anode platinum-titanium mesh was evenly placed around the GH4169 nickel-based high-temperature alloy, and the distance between the anode and the cathode nickel-based high-temperature alloy was 15cm. During the electrodeposition process, a filter pump was used to circulate and filter the plating solution.
[0075] Step 4: subjecting the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy obtained in step 3 to dehydrogenation annealing treatment; the temperature of the annealing dehydrogenation treatment is 250° C. and the time is 3 hours.
[0076] Figure 5 This is the SEM image of the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy obtained in this embodiment. Figure 5 It can be seen that the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy in this embodiment is continuous, the surface condition is good, and there is no peeling or cracking.
[0077] Figure 6 is a cross-sectional SEM image of the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy obtained in this embodiment. Figure 6 It can be seen that the thickness of the platinum layer on the surface of the GH4169 nickel-based high-temperature alloy in this embodiment is 5.59 μm, and the platinum layer and the GH4169 nickel-based high-temperature alloy have good interface bonding.
[0078] Embodiment 3:
[0079] The electrolyte provided in this embodiment for electrodepositing a platinum layer on the surface of a nickel-based high-temperature alloy is prepared by mixing tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecylbenzene sulfonate and deionized water. The content of each component in the electrolyte is: 3 g / L (in terms of platinum) of tetraamine platinum hydrogen phosphate, 30 g / L of disodium ethylenediaminetetraacetate, 20 g / L of sodium phosphate, 1.0 g / L of sodium dodecylbenzene sulfonate, an appropriate amount of sodium hydroxide to adjust the pH, and the balance is deionized water.
[0080] The electrodeposition method provided in this embodiment comprises the following steps:
[0081] Step 1: The surface of the DD419 nickel-based high-temperature alloy is sandblasted and degreased in sequence; the sand used for sandblasting is glass beads, the sand size is 200 mesh, the sandblasting pressure is 0.15 MPa, the sandblasting angle is 80°, the sandblasting distance is 90 mm, and the sandblasting times are 6 times.
[0082] Step 2: Place the sandblasted DD419 nickel-based high-temperature alloy in a degreasing tank for electrolytic degreasing. The degreasing liquid used is composed of 20g / L sodium hydroxide, 30g / L sodium phosphate, 40g / L sodium carbonate, and the rest is deionized water. Electrolytic degreasing process parameters: voltage is 2V, temperature is room temperature, and time is 2min. Cathode degreasing is used, and titanium mesh is used as anode. Then rinse with deionized water.
[0083] Step 3: Place the washed DD419 nickel-based high-temperature alloy in an electrolyte with a pH of 9.5, an electrolyte temperature of 90°C, and a current density of 0.75A / dm 2 Electrodeposition was carried out for 0.5h under the conditions of , and the concentration of platinum in the plating solution was maintained at 10g / L calculated as platinum by adding tetraamine platinum hydrogen phosphate during the electroplating process to obtain a platinum layer on the surface of DD419 nickel-based high-temperature alloy; the pH value was adjusted by sodium hydroxide; the anode used in the electroplating process was a platinum-plated titanium mesh, and the cathode was a DD419 nickel-based high-temperature alloy workpiece. The anode platinum-plated titanium mesh was evenly placed around the DD419 nickel-based high-temperature alloy, and the distance between the anode and the cathode nickel-based high-temperature alloy was 12cm; a filter pump was used to circulate and filter the plating solution during the electroplating process.
[0084] Step 4: subjecting the DD419 nickel-based high-temperature alloy platinum layer obtained in step 3 to dehydrogenation annealing; the temperature of the dehydrogenation annealing is 400° C. and the time is 2 h.
[0085] Figure 7 is a cross-sectional SEM image of the platinum layer on the surface of the DD419 nickel-based high-temperature alloy obtained in this embodiment. Figure 7 It can be seen that in this embodiment, the platinum layer on the surface of the DD419 nickel-based high-temperature alloy is continuous, the thickness of the platinum layer is 3.49 μm, and the interface between the platinum layer and the DD419 nickel-based high-temperature alloy substrate is well bonded.
[0086] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
[0087] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the term "comprises" or any other variant thereof is intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprises a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0088] In the above embodiments, the descriptions of directions such as “upper” and “lower” are all based on the drawings.
[0089] The above description of the disclosed embodiments enables those skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0090] Thus, the present invention will not be limited to the embodiments shown herein but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A plating solution for electroplating a platinum layer on the surface of a nickel-based high-temperature alloy, It is characterized in that The invention comprises tetraamine platinum hydrogen phosphate, disodium ethylenediaminetetraacetate, sodium phosphate, sodium dodecyl sulfate, sodium hydroxide and deionized water; in terms of platinum, the concentration of tetraamine platinum hydrogen phosphate is 2g / L-10g / L; the concentration of disodium ethylenediaminetetraacetate is 20g / L-40g / L; the concentration of sodium phosphate is 10g / L-30g / L; the concentration of sodium dodecyl sulfate is 0.5g / L-1g / L, the pH value of the plating solution is 9.5-10.5, and the balance is deionized water.
2. An electrodeposition method, It is characterized in that include: Clean the surface of nickel-based high-temperature alloy; The plating solution of claim 1 is used to electro-deposit the surface of the nickel-based high-temperature alloy to prepare a platinum layer on the surface of the nickel-based high-temperature alloy.
3. The electrodeposition method according to claim 2, It is characterized in that The cleaning of the surface of the nickel-based high-temperature alloy comprises sequentially performing sandblasting, electrolytic degreasing and water washing.
4. The electrodeposition method according to claim 3, It is characterized in that The sand used for sand blasting is white corundum sand and / or glass beads; the pressure of the sand blasting is 0.1MPa-0.3MPa, the sand blasting angle is 70°-90°, the sand blasting distance is 90mm-150mm, and the time is 2min-6min.
5. The electrodeposition method according to claim 3, It is characterized in that The degreasing liquid used in the electrolytic degreasing includes sodium hydroxide, sodium phosphate, sodium carbonate and deionized water; 10g / L to 20g / L of sodium hydroxide, 20g / L to 40g / L of sodium phosphate, and 10g / L to 20g / L of sodium carbonate; during the electrolytic degreasing process, the voltage is 2V, the temperature is maintained at room temperature, and the time is 2 to 5 minutes; cathode degreasing is adopted, and titanium mesh is selected as the anode.
6. The electrodeposition method according to claim 2, It is characterized in that During the electroplating process, the plating solution temperature is 85°C to 90°C, the pH value is 9.5 to 10.5, and the electroplating current density is 0.5A / dm 2 ~2A / dm 2 , electrodeposition time is 0.5h~2h.
7. The electrodeposition method according to claim 2, It is characterized in that During the electrodeposition process, tetraammine platinum hydrogen phosphate solution is added to maintain the concentration of platinum in the plating solution.
8. The electrodeposition method according to claim 7, It is characterized in that In the tetraamine platinum hydrogen phosphate solution, the concentration of the tetraamine platinum hydrogen phosphate solution is 2 g / L to 10 g / L, calculated as platinum.
9. The electrodeposition method according to claim 2, It is characterized in that During the electrodeposition process, gas stirring or cathode movement is applied, and during the electrodeposition process, a filter pump is used to circulate and filter the plating solution.
10. The electrodeposition method according to claim 2, It is characterized in that The platinum layer on the surface of the nickel-based high-temperature alloy is subjected to a dehydrogenation annealing treatment, wherein the temperature of the dehydrogenation annealing treatment is 200° C. to 400° C. and the time is 2 h to 4 h.
Citation Information
Patent Citations
Process for manufacturing an electrolytic bath for the production of a platinum-based metallic sublayer on a metallic substrate
CN104271811A
Electroplating solution for electroplating platinum layer on surface of nickel-based superalloy and electroplating method of plating solution
CN108130566A
Cited By
Current collector and preparation method therefor, secondary battery and electric device
WO2026171253A1