Manufacturing method of heterogeneous bonding structure

By forming a transition layer with a lattice mismatch of less than or equal to 5% on SiC and Si wafers and bonding, the problem of poor interface quality caused by lattice mismatch in the existing technology is solved, and high-quality heterogeneous products are achieved. The qualitative bonding structure improves device performance.

CN118763065APending Publication Date: 2024-10-11INST OF MICROELECTRONICS CHINESE ACAD OF SCI LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410870874.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

The existing SiC and Si wafer bonding process does not fully consider the lattice mismatch problem, resulting in poor quality of the bonding interface, large interface thermal resistance and many interface states, which affects the performance of Si functional layer devices.

Method used

By forming transition layers with a lattice mismatch of less than or equal to 5% on the first substrate and the second substrate, using pulse laser deposition technology to form SiNX and SiO2 layers, and performing room temperature bonding and annealing treatments to reduce the lattice distortion and interface defects to improve interface bonding quality.

Benefits of technology

It effectively reduces defects and lattice mismatch at the interface of the heterogeneous bonding structure, improves the quality of interface bonding, and ensures the performance of the heterogeneous bonding structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118763065A_ABST
    Figure CN118763065A_ABST
Patent Text Reader

Abstract

The invention discloses a manufacturing method of a heterogeneous bonding structure, relates to the technical field of semiconductors, and aims to solve the problem that the bonding quality of an interface is affected due to the fact that lattice mismatch at the interface of the finally obtained heterogeneous bonding structure is serious. The manufacturing method of the heterogeneous bonding structure comprises the following steps: providing a first substrate and a second substrate; forming a first transition layer on the first substrate to obtain a first structure; the lattice mismatch degree between the first transition layer and the first substrate is smaller than or equal to 5%; forming a second transition layer on the second substrate to obtain a second structure; the lattice mismatch degree between the second transition layer and the second substrate is less than or equal to 5%; the lattice mismatch degree between the first transition layer and the second transition layer is less than or equal to 5%; and bonding the first transition layer included in the first structure and the second transition layer included in the second structure to obtain the heterogeneous bonding structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to a method for manufacturing a heterogeneous bonding structure. Background Art

[0002] At present, heterogeneous bonding processes are usually used to integrate different types of semiconductor materials. Silicon carbide (SiC) wafers and silicon (Si) wafers can be combined through a bonding process to obtain silicon carbide on silicon wafer materials.

[0003] The existing SiC and Si wafer bonding process uses a direct bonding process, that is, directly bonding SiC and Si wafer materials, without fully considering the lattice mismatch between wafers, resulting in poor quality of the bonding interface, large interface thermal resistance and more interface states, which seriously affects the performance of Si functional layer devices. Therefore, it is urgent to improve the bonding process of SiC and Si wafers to reduce the interface lattice mismatch and improve the interface bonding quality. Summary of the invention

[0004] The object of the present invention is to provide a method for manufacturing a heterogeneous bonding structure, which is used to reduce the interface lattice mismatch and improve the interface bonding quality.

[0005] In order to achieve the above object, the present invention provides a method for manufacturing a heterogeneous bonding structure. The method for manufacturing a heterogeneous bonding structure comprises:

[0006] First, a first substrate and a second substrate are provided;

[0007] Next, a first transition layer is formed on the first substrate to obtain a first structure; the lattice mismatch between the first transition layer and the first substrate is less than or equal to 5%;

[0008] Next, forming a second transition layer on the second substrate to obtain a second structure; the lattice mismatch between the second transition layer and the second substrate is less than or equal to 5%;

[0009] The lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%;

[0010] The first transition layer included in the first structure and the second transition layer included in the second structure are bonded to obtain a heterogeneous bonding structure.

[0011] Compared with the prior art, in the method for manufacturing a heterogeneous bonding structure provided by the present invention, since the lattice mismatch between the first transition layer and the first substrate is less than or equal to 5%, the lattice matching between the first substrate and the first transition layer can be improved, and the first transition layer can be well grown on the first substrate, thereby reducing or avoiding the lattice distortion. Further, since the lattice mismatch between the second transition layer and the second substrate is less than or equal to 5%, the second transition layer can be well grown on the second substrate, thereby reducing or avoiding the lattice distortion. Further, since the lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%, the first transition layer and the second transition layer have a high lattice matching, and the lattice mismatch at the first transition layer and the second transition layer can be reduced, and the precision bonding between the first transition layer and the second transition layer can be achieved, thereby reducing or avoiding the lattice distortion. In summary, the method for manufacturing a heterogeneous bonding structure provided by the present invention can reduce defects at the interface between the first substrate and the first transition layer, defects at the interface between the second substrate and the second transition layer, and defects and lattice mismatch at the interface between the first transition layer and the second transition layer, thereby reducing defects at the interface of the heterogeneous bonding structure finally obtained, improving the interface bonding quality, and ensuring the performance of the heterogeneous bonding structure.

[0012] In one implementation, the first substrate includes a SiC layer, and the first transition layer is a SiN X SiN layer is formed on the SiC layer X Layer; wherein x is greater than or equal to 1 and less than or equal to 4 / 3;

[0013] The second substrate includes a Si layer, and the second transition layer is a SiO2 layer; the SiO2 layer is formed on the Si layer.

[0014] In one implementation, the first substrate is a SiC substrate, and the SiC substrate is a 4H-SiC substrate;

[0015] The second substrate is a bulk Si substrate or an SOI substrate; the SOI substrate comprises a stacked Si layer, a buried oxide layer and a silicon substrate, and a second transition layer is formed on a side of the Si layer away from the buried oxide layer.

[0016] In one implementation, before forming a first transition layer on the first substrate to obtain the first structure, the method for manufacturing the heterogeneous bonding structure further includes: -5 Pa, plasma cleaning or ultrasonic cleaning is performed on the first substrate by radio frequency power supply, and the cleaning time is greater than or equal to 15 minutes and less than or equal to 40 minutes;

[0017] Before forming a second transition layer on the second substrate to obtain the second structure, the method for manufacturing the heterogeneous bonding structure also includes: ultrasonically cleaning the second substrate using deionized water, acetone, alcohol, and deionized water in sequence, with each cleaning time being greater than or equal to 15 minutes and less than or equal to 40 minutes.

[0018] In one implementation, forming a first transition layer on a first substrate to obtain a first structure includes:

[0019] Using pulsed laser deposition technology, SiN is formed on the first substrate. X Layer; SiN X The thickness of the layer is greater than or equal to 1 nm and less than or equal to 15 nm.

[0020] In one implementation, forming a second transition layer on the second substrate to obtain a second structure includes:

[0021] A SiO2 layer is formed on the Si layer included in the second substrate by using pulse laser deposition technology; the thickness of the SiO2 layer is greater than or equal to 1 nm and less than or equal to 15 nm.

[0022] In one implementation, bonding the first transition layer included in the first structure and the second transition layer included in the second structure to obtain a heterogeneous bonding structure includes:

[0023] SiN X The layer and the SiO2 layer are bonded at room temperature to obtain a pre-treated heterogeneous bonding structure;

[0024] performing an annealing treatment on the pretreated heterogeneous bonding structure to obtain a heterogeneous bonding structure;

[0025] The parameters of the annealing treatment include: an annealing temperature greater than or equal to 300° C. and less than or equal to 1200° C., and an annealing time greater than or equal to 1 hour and less than or equal to 24 hours.

[0026] In one implementation, after the pre-treated heterogeneous bonding structure is annealed, the method for manufacturing the heterogeneous bonding structure further includes:

[0027] The first substrate and the second substrate are thinned to obtain a heterogeneous bonding structure.

[0028] In one implementation, when the second substrate is an SOI substrate, the SOI substrate includes a stacked Si layer, a buried oxide layer and a silicon substrate, and a second transition layer is formed on the Si layer, after the pre-treated heterogeneous bonding structure is annealed, the method for manufacturing the heterogeneous bonding structure further includes:

[0029] The buried oxide layer and the silicon substrate are removed by a method combining wet etching and grinding to expose the Si layer included in the second substrate.

[0030] In one implementation, before bonding the first transition layer included in the first structure and the second transition layer included in the second structure, the method for manufacturing the heterogeneous bonding structure further includes:

[0031] The first structure and the second structure are cleaned separately. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0033] Figure 1 Schematic diagram of the structure of the first substrate and the first transition layer in an embodiment of the present invention;

[0034] Figure 2 This is a schematic diagram of the structure of the second substrate and the second transition layer in an embodiment of the present invention;

[0035] Figure 3 A schematic diagram of the structure of the first structure and the second structure in an embodiment of the present invention;

[0036] Figure 4 A schematic diagram of processing the first structure and the second structure by a method combining wet etching and grinding in an embodiment of the present invention;

[0037] Figure 5 Schematic diagram of the structure of the heterogeneous bonding structure in an embodiment of the present invention.

[0038] Reference numerals:

[0039] 1-first substrate, 2-second substrate, 20-Si layer, 21-buried oxide layer, 22-silicon substrate; 3-first transition layer, 4-second transition layer. DETAILED DESCRIPTION

[0040] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0041] It should be noted that when an element is referred to as being "fixed to" or "disposed on" another element, it can be directly on the other element or indirectly on the other element. When an element is referred to as being "connected to" another element, it can be directly connected to the other element or indirectly connected to the other element.

[0042] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. The meaning of "several" is one or more, unless otherwise clearly and specifically defined.

[0043] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by the terms "up", "down", "front", "back", "left", "right", etc. are based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction, and therefore cannot be understood as a limitation on the present invention.

[0044] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0045] Silicon On Silicon Carbide (SOS) is an advanced semiconductor process technology, mainly used to prepare high-power, high-temperature electronic devices. In this technology, a thin silicon layer is heterogeneously bonded to a silicon carbide substrate, and various electronic devices can be manufactured in the silicon layer through standard CMOS processes. Because silicon carbide (SiC) has excellent physical and chemical properties, such as high thermal conductivity and excellent thermal stability, it has become an ideal substrate material for power electronic devices. Compared with growing silicon structures on silicon substrates, silicon structures on silicon carbide can operate at higher temperatures and the devices consume less energy.

[0046] However, despite the huge advantages and potential of SOS technology, there are also some challenges. Due to the lattice mismatch between silicon and silicon carbide and the mismatch of thermal expansion coefficient, it is a big problem to directly grow a high-quality single-crystalline silicon layer on a SiC substrate, and defects and stress are easily generated in the silicon layer. Therefore, the quality of the interface between silicon and silicon carbide has a great influence on the performance of the device, so how to achieve a high-quality Si / SiC interface is also an important task.

[0047] Heterogeneous bonding is a semiconductor manufacturing process that is used to connect two or more different semiconductor materials to achieve the desired device characteristics, which is crucial for integrated microelectronic devices. However, due to the lattice misalignment and thermal expansion coefficient mismatch between different semiconductor materials, direct bonding often produces a large number of defects at the interface, affecting the performance of the device.

[0048] In addition to the prior art method of bonding two semiconductor structures described in the background section, there are two other methods.

[0049] The second method is to use an accelerated electron beam of argon to activate the surface of SiC, remove pollutants and oxide layers on its surface, and keep the surface of SiC to be bonded clean and flat. Then, a layer of Si layer about 10nm thick is deposited on the surface of SiC by sputtering. Then, another Si layer and the surface of SiC are activated again by an accelerated electron beam of argon. Finally, Si-SiC bonding is achieved under an external pressure of 4MPa at room temperature.

[0050] However, this method actually uses a layer of silicon as an intermediate layer to complete the bonding, but there is still a lattice mismatch problem between silicon and silicon carbide, and it is difficult to ensure the quality of the 10nm silicon layer during the deposition process, which greatly affects the interface quality.

[0051] The third type: The existing technology proposes a silicon-silicon carbide bonding technology based on graphene composite slurry as the intermediate layer. The results show that with the increase of sintering temperature, the graphene composite slurry is more densely bonded, and Si-SiC bonding is achieved under the conditions of 600N and 200°C, with a bonding strength of 3.4MPa.

[0052] The graphene composite slurry is prepared by mixing a binder with graphene powder and a polymer solvent, etc. The addition of the binder will increase the bonding strength, but the electrical conductivity and thermal conductivity of the binder are very poor, which will reduce the electrical conductivity and thermal conductivity of the graphene composite slurry, resulting in a decrease in device performance.

[0053] In order to solve at least one of the above technical problems, the present invention provides a method for manufacturing a heterogeneous bonding structure. Figures 1 to 5 , the method for manufacturing the above-mentioned heterogeneous bonding structure comprises:

[0054] Step 101: Provide a first substrate and a second substrate.

[0055] The first substrate and the second substrate may be in the form of a wafer or a chip. For example, when the first substrate is a wafer, the second substrate is a chip. Alternatively, when the first substrate is a chip, the second substrate is a wafer. Alternatively, both the first substrate and the second substrate are wafers. Alternatively, both the first substrate and the second substrate are chips. Further, the first substrate and the second substrate are made of different types of semiconductor materials. Further, the production time of the first substrate and the second substrate should be within 2 months to prevent the substrate properties from changing due to time, so as to ensure the quality of the heterogeneous bonding structure obtained later.

[0056] Step 102: In the range less than or equal to 1×10 -5 Pa environment, the first substrate is plasma cleaned or ultrasonically cleaned by a radio frequency power supply, and the cleaning time is greater than or equal to 15 minutes and less than or equal to 40 minutes; for example, the cleaning time is 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, etc.

[0057] When adopting the above technical solution, a semiconductor process is used to clean the first substrate in a near-vacuum environment to ensure the quality and cleanliness of the bonding surface of the first substrate (i.e., the surface on which the first transition layer needs to be formed later), reduce or eliminate the impurity content of the bonding surface of the first substrate, and ensure the quality of subsequent bonding.

[0058] Step 103: ultrasonically clean the second substrate using deionized water, acetone, alcohol, and deionized water in sequence, with each cleaning time being greater than or equal to 15 minutes and less than or equal to 40 minutes. For example, the cleaning time is 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, or 40 minutes.

[0059] Exemplarily, the second substrate is first cleaned with deionized water using an ultrasonic cleaning method to remove inorganic impurities on the second substrate. Next, acetone is used to remove organic impurities on the second substrate. Next, alcohol cleaning is used to remove acetone. Next, deionized water cleaning is used to remove alcohol.

[0060] When adopting the above technical solution, the second substrate is cleaned by a semiconductor process to ensure the quality and cleanliness of the bonding surface of the second substrate (i.e., the surface on which the second transition layer needs to be formed later), reduce or eliminate the impurity content of the bonding surface of the second substrate, and ensure the quality of subsequent bonding.

[0061] Step 104: See Figure 1, forming a first transition layer 3 on the first substrate 1 to obtain a first structure; the lattice mismatch between the first transition layer 3 and the first substrate 1 is less than or equal to 5%; illustratively, the lattice mismatch between the first transition layer and the first substrate can be 0.3%, 1%, 2%, 3.3%, 4% or 5%, etc. It should be understood that the lattice mismatch between the first transition layer and the first substrate is equal to the difference in lattice constants between the first transition layer and the first substrate divided by the lattice constant of the first substrate.

[0062] As a possible implementation, see Figure 1 The first substrate 1 includes a SiC layer, and the first transition layer 3 is SiN X layer, forming SiN on the SiC layer X Where x is greater than or equal to 1 and less than or equal to 4 / 3. For example, SiN X It can be SiN or Si3N4.

[0063] There are four C atoms around each Si atom in SiC, and each Si (or C) atom is bonded to the surrounding C (or Si) atoms through a directional strong tetrahedral SP3 bond. X There are four N atoms around each Si atom in SiC, and each Si (or N) atom is bonded to the surrounding N (or Si) atoms through a directional strong tetrahedral SP3 bond. X With the same lattice structure, SiN can be well grown on the SiC layer. X layer to reduce or avoid lattice distortion.

[0064] In an optional manner, the first substrate is a SiC substrate. Preferably, the SiC substrate is a 4H-SiC substrate. X Both are hexagonal crystals and have similar atomic compositions, so 4H-SiC and SiN X It has a very high lattice matching degree. At this time, it can be achieved that SiN is well grown on the 4H-SiC substrate. X layer, thereby greatly reducing or avoiding lattice distortion and ensuring that the 4H-SiC substrate and SiN X In the embodiment of the present invention, the first substrate is a 4H-SiC standard wafer. The production time of the 4H-SiC standard wafer should be within 2 months to prevent the wafer properties from changing due to time, so as to ensure the quality of the heterogeneous bonding structure obtained later.

[0065] More preferably, SiN XThe layer is a Si3N4 layer. Both SiC and Si3N4 are hexagonal systems, and except for Si, the C atomic radius is 67pm and the N atomic radius is 62pm, which are very close. At this time, the lattice matching between the first substrate and the first transition layer can be further improved, and the first transition layer can be well grown on the first substrate, thereby further reducing or avoiding lattice distortion.

[0066] In an alternative approach, see Figure 1 , forming a first transition layer 3 on the first substrate 1 to obtain a first structure includes: forming SiN on the first substrate 1 by pulse laser deposition technology X Layer; SiN X The thickness of the layer is greater than or equal to 1 nm and less than or equal to 15 nm. For example, SiN X The thickness of the layer is 1 nm, 2 nm, 5 nm, 8 nm, 10 nm, 12 nm, 14 nm or 15 nm, etc. SiN X Too thin a layer is not conducive to SiN X The uniform growth of the layer cannot be precisely controlled. X If the thickness of the layer is too thick, it will introduce significant changes in interface properties, such as reducing thermal conductivity. X The thickness direction of the layer is consistent with the direction from the first substrate 1 to the first transition layer 3 .

[0067] The first substrate comprises a SiC layer, and the SiC layer has a Si surface and a C surface. In combination with the above-described step 102, only the Si surface of the SiC layer may be cleaned, or the entire SiC layer may be cleaned, as long as the cleanliness of the bonding surface is ensured.

[0068] In the embodiment of the present invention, a pulse laser deposition technology (PLD) is used to uniformly form a SiN layer with a thickness of 10 nm on a 4H-SiC standard wafer. X layer.

[0069] Step 105: See Figure 2 , a second transition layer 4 is formed on the second substrate 2 to obtain a second structure; the lattice mismatch between the second transition layer and the second substrate is less than or equal to 5%. Exemplarily, the lattice mismatch between the second transition layer and the second substrate can be 0.3%, 1%, 2%, 3.3%, 4% or 5%, etc. It should be understood that the lattice mismatch between the second transition layer and the second substrate is equal to the difference in lattice constants between the second transition layer and the second substrate divided by the lattice constant of the second substrate.

[0070] The lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%. For example, the lattice mismatch between the first transition layer and the second transition layer can be 0.3%, 1%, 2%, 3.3%, 4% or 5%, etc.

[0071] As a possible implementation, the second substrate includes a Si layer, the second transition layer is a SiO2 layer, and the SiO2 layer is formed on the Si layer. SiO2, as a product formed by natural oxidation of Si, has extremely good lattice adaptability to Si and a very close thermal expansion coefficient. After the SiO2 layer is formed on the Si layer, the Si layer and the SiO2 layer can be precisely bonded, thereby greatly reducing or avoiding lattice distortion, thereby ensuring the bonding quality of the Si layer and the SiO2 layer.

[0072] Further, combined with the above description, when the first transition layer is a Si3N4 layer, since both SiO2 and Si3N4 are hexagonal crystal systems, and except for Si, the O atomic radius of 60pm and the N atomic radius of 62pm are very close, precise bonding between the first transition layer and the second transition layer can be further achieved, thereby reducing or avoiding lattice distortion.

[0073] In an alternative approach, see Figure 2 , the second substrate 2 is a bulk Si substrate or an SOI substrate. The SOI substrate includes a stacked Si layer 20, a buried oxide layer 21 (Buried Oxide, abbreviated as BOX) and a silicon substrate 22 (Substrate, abbreviated as SUB), and a second transition layer 4 is formed on a side of the Si layer away from the buried oxide layer. When the second substrate is an SOI substrate, it is beneficial to use etching technology to quickly remove the silicon substrate and the buried oxide layer in the subsequent thinning step, leaving only a thin Si layer for chemical mechanical polishing (CMP).

[0074] Combined with the above description, in the embodiment of the present invention, the first substrate and the second substrate are both wafers. Specifically, the second substrate is a SOI standard wafer. Among them, the production time of the SOI standard wafer should be within 2 months to prevent the wafer properties from changing due to time, so as to ensure the quality of the heterogeneous bonding structure obtained later.

[0075] In an alternative approach, see Figure 2, forming a second transition layer 4 on the second substrate 2 to obtain the second structure includes: using pulsed laser deposition technology to form a SiO2 layer on the Si layer included in the second substrate 2; the thickness of the SiO2 layer is greater than or equal to 1nm and less than or equal to 15nm. For example, the thickness of the SiO2 layer is 1nm, 2nm, 5nm, 8nm, 10nm, 12nm, 14nm or 15nm. If the thickness of the SiO2 layer is too thin, it will be unfavorable for the uniform growth of the SiO2 layer and cannot be accurately controlled. If the thickness of the SiO2 layer is too thick, it will introduce obvious changes in interface properties, such as reducing thermal conductivity. It should be noted that the thickness direction of the above-mentioned SiO2 layer is consistent with the direction from the second substrate 2 to the second transition layer 4.

[0076] In the embodiment of the present invention, a pulsed laser deposition technology is used to form a SiO2 layer with a thickness of 10 nm on the Si layer included in the SOI standard wafer.

[0077] Step 106: Clean the first structure and the second structure respectively to remove impurities on the bonding surface of the first structure and the bonding surface of the second structure.

[0078] Specifically, less than or equal to 1×10 -5 Pa environment, the first structure is plasma cleaned or ultrasonically cleaned by a radio frequency power supply, and the cleaning time is greater than or equal to 15 minutes and less than or equal to 40 minutes; for example, the cleaning time is 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes or 40 minutes, etc.

[0079] The second structure is ultrasonically cleaned using deionized water, acetone, alcohol, and deionized water in sequence, and each cleaning time is greater than or equal to 15 minutes and less than or equal to 40 minutes. For example, the cleaning time is 15 minutes, 20 minutes, 25 minutes, 30 minutes, 35 minutes, or 40 minutes.

[0080] Step 107: See Figure 3 , the first transition layer 3 included in the first structure and the second transition layer 4 included in the second structure are bonded to obtain a heterogeneous bonding structure.

[0081] Specifically, step 107.1: when the first transition layer is SiN X When the second transition layer is SiO2, SiN X The layer and the SiO2 layer are bonded at room temperature to obtain a pre-treated heterogeneous bonding structure;

[0082] When the above technical solution is adopted, due to the SiN X Both SiO2 and SiN are hexagonal crystals with similar atomic composition. X It has a very high lattice matching degree with SiO2. At this time, SiNX The precise bonding of the SiO2 layer and the SiO2 layer can greatly reduce or avoid lattice distortion, reduce defects at the interface of the heterogeneous bonded structure, and thus ensure the performance of the heterogeneous bonded structure.

[0083] Exemplarily, the second structure is inverted on the first structure, and SiN X The layer and the SiO2 layer are hydrophilically bonded at room temperature to obtain a pretreated heterogeneous bonding structure.

[0084] The normal temperature in the above-mentioned normal temperature hydrophilic bonding is generally 25°C.

[0085] Hydrophilic bonding is a common bonding method in the prior art, and the general steps are as follows: 1. Surface cleaning and hydrophilization: In addition to the basic cleaning steps, a specific chemical treatment (nitric acid or hydrochloric acid) is used to increase the hydrophilicity of the surface, which helps to form abundant hydroxyl groups on the surface of the intermediate layer. 2. Contact pressing: Under clean room temperature conditions, the wafers are contacted and then gently pressure is applied to ensure good contact between the two. 3. Annealing to convert hydrogen bonds into covalent bonds: Annealing treatment is performed to promote the conversion of hydrogen bonds between hydroxyl groups at the interface into more stable covalent bonds.

[0086] Step 107.2: performing annealing treatment on the pre-treated heterogeneous bonding structure to obtain a heterogeneous bonding structure;

[0087] The parameters of the annealing treatment include: an annealing temperature greater than or equal to 300° C. and less than or equal to 1200° C., and an annealing time greater than or equal to 1 hour and less than or equal to 24 hours. For example, the annealing temperature is 300° C., 350° C., 400° C., 450° C., 500° C., 550° C., 600° C., or 1200° C., etc. The annealing time is 1 hour, 8 hours, 10 hours, 15 hours, 18 hours, 20 hours, 22 hours, 23 hours, or 24 hours, etc.

[0088] If the annealing temperature is too low or the annealing time is too short, it will lead to insufficient energy, reduce the quality of the covalent bond formed, and make the bonding quality at the interface worse. If the annealing temperature is too high or the annealing time is too long, the wafer may crack and be damaged.

[0089] In an optional manner, after the pre-treated heterogeneous bonding structure is annealed, if the thickness of the obtained structure is relatively thick, the first substrate and the second substrate are thinned to obtain a heterogeneous bonding structure with a thickness that meets actual requirements.

[0090] Exemplarily, the first substrate and the second substrate are thinned by using a chemical mechanical polishing (CMP) technique.

[0091] In an alternative approach, see Figure 4 and Figure 5 When the second substrate 2 is an SOI substrate, the SOI substrate includes a stacked Si layer 20, a buried oxide layer 21 and a silicon substrate 22, and a second transition layer 4 is formed on a side of the Si layer 20 away from the buried oxide layer, after the pre-treated heterogeneous bonding structure is annealed, the method for manufacturing the heterogeneous bonding structure further includes: removing the buried oxide layer 21 and the silicon substrate 22 by a combination of wet etching and grinding to expose the Si layer 20 included in the second substrate 2. It should be noted that if the thickness of the obtained structure is still relatively thick after the Si layer included in the second substrate 2 is exposed, the first substrate 1 and the second substrate 2 are thinned to obtain a heterogeneous bonding structure with a thickness that meets actual needs.

[0092] Combined with the above description, the first transition layer and the second transition layer are used as buffer layers for the bonding surfaces of the SiC wafer and the SOI wafer. Through this buffer layer, the lattice constant and the thermal expansion coefficient can be gradually changed, thereby reducing the defects generated at the bonding interface, thereby effectively solving the lattice mismatch problem between the SiC wafer and the SOI wafer, reducing the lattice distortion at the interface between the SiC wafer and the SOI wafer, thereby reducing stress and defects, enhancing the bonding quality, and improving the problems of large interface thermal resistance and more interface states. Furthermore, the heterogeneous bonding structure finally obtained in the embodiment of the present invention is a multilayer structure of Si-SiO2-SiNx-SiC, which can form a step-by-step buffer for the lattice mismatch and enhance the interface quality.

[0093] In the method for manufacturing a heterogeneous bonding structure provided by an embodiment of the present invention, since the lattice mismatch between the first transition layer and the first substrate is less than or equal to 5%, the lattice matching between the first substrate and the first transition layer can be improved, and the first transition layer can be well grown on the first substrate, thereby reducing or avoiding the lattice distortion. Further, since the lattice mismatch between the second transition layer and the second substrate is less than or equal to 5%, the second transition layer can be well grown on the second substrate, thereby reducing or avoiding the lattice distortion. Further, since the lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%, the first transition layer and the second transition layer have a high lattice matching, and the lattice mismatch at the first transition layer and the second transition layer can be reduced, and the precision bonding between the first transition layer and the second transition layer can be achieved, thereby reducing or avoiding the lattice distortion. In summary, the method for manufacturing a heterogeneous bonding structure provided by the present invention can reduce defects at the interface between the first substrate and the first transition layer, defects at the interface between the second substrate and the second transition layer, and defects and lattice mismatch at the interface between the first transition layer and the second transition layer, thereby reducing defects at the interface of the heterogeneous bonding structure finally obtained, improving the interface bonding quality, and ensuring the performance of the heterogeneous bonding structure.

[0094] In addition, compared to the prior art described in the background technology section, the manufacturing method provided in the embodiment of the present invention simplifies the surface treatment before bonding the first substrate and the second substrate. Further, compared to the second method, silicon is no longer used as the intermediate layer to complete the bonding, but the first transition layer and the second transition layer are selected (the lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%), which solves the lattice mismatch problem between silicon and silicon carbide. Since silicon is no longer used as the intermediate layer, there is no need to deposit a 10nm silicon layer, and then there is no need to consider the impact of the quality of the 10nm silicon layer on the interface quality. Furthermore, compared to the third method, the embodiment of the present invention no longer uses graphene composite slurry, so there is no need to consider a series of problems caused by graphene composite slurry.

[0095] In the description of the above embodiments, specific features, structures, materials or characteristics may be combined in a suitable manner in any one or more embodiments or examples.

[0096] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.

Claims

1. A method for manufacturing a heterogeneous bonding structure, characterized in that: include: providing a first substrate and a second substrate; forming a first transition layer on the first substrate to obtain a first structure; The lattice mismatch between the first transition layer and the first substrate is less than or equal to 5%; forming a second transition layer on the second substrate to obtain a second structure; wherein the lattice mismatch between the second transition layer and the second substrate is less than or equal to 5%; The lattice mismatch between the first transition layer and the second transition layer is less than or equal to 5%; The first transition layer included in the first structure and the second transition layer included in the second structure are bonded to obtain a heterogeneous bonding structure.

2. The method for manufacturing a heterogeneous bonding structure according to claim 1, characterized in that: The first substrate includes a SiC layer, and the first transition layer is a SiN X forming the SiN layer on the SiC layer X Layer; wherein x is greater than or equal to 1 and less than or equal to 4 / 3; The second substrate includes a Si layer, and the second transition layer is a SiO2 layer; the SiO2 layer is formed on the Si layer.

3. The method for manufacturing a heterogeneous bonding structure according to claim 1 or 2, characterized in that: The first substrate is a SiC substrate, and the SiC substrate is a 4H-SiC substrate; The second substrate is a bulk Si substrate or an SOI substrate; the SOI substrate comprises a stacked Si layer, a buried oxide layer and a silicon substrate, and the second transition layer is formed on a side of the Si layer away from the buried oxide layer.

4. The method for manufacturing a heterogeneous bonding structure according to claim 1, characterized in that: Before forming a first transition layer on the first substrate to obtain a first structure, the method for manufacturing the heterogeneous bonding structure further comprises: -5 Pa, performing plasma cleaning or ultrasonic cleaning on the first substrate by radio frequency power supply, and the cleaning time is greater than or equal to 15 minutes and less than or equal to 40 minutes; Before forming a second transition layer on the second substrate to obtain a second structure, the method for manufacturing the heterogeneous bonding structure also includes: ultrasonically cleaning the second substrate using deionized water, acetone, alcohol, and deionized water in sequence, with each cleaning time being greater than or equal to 15 minutes and less than or equal to 40 minutes.

5. The method for manufacturing a heterogeneous bonding structure according to claim 2, characterized in that: Forming a first transition layer on the first substrate to obtain a first structure includes: A pulsed laser deposition technique is used to form SiN on the first substrate. X layer; the SiN X The thickness of the layer is greater than or equal to 1 nm and less than or equal to 15 nm.

6. The method for manufacturing a heterogeneous bonding structure according to claim 2, characterized in that: Forming a second transition layer on the second substrate to obtain a second structure comprises: A SiO2 layer is formed on the Si layer included in the second substrate by using pulse laser deposition technology; the thickness of the SiO2 layer is greater than or equal to 1 nm and less than or equal to 15 nm.

7. The method for manufacturing a heterogeneous bonding structure according to claim 2, characterized in that: Bonding the first transition layer included in the first structure and the second transition layer included in the second structure to obtain a heterogeneous bonding structure comprises: The SiN X The layer and the SiO2 layer are bonded at room temperature to obtain a pre-treated heterogeneous bonding structure; Performing annealing treatment on the pretreated heterogeneous bonding structure to obtain the heterogeneous bonding structure; The parameters of the annealing treatment include: an annealing temperature greater than or equal to 300° C. and less than or equal to 1200° C., and an annealing time greater than or equal to 1 hour and less than or equal to 24 hours.

8. The method for manufacturing a heterogeneous bonding structure according to claim 7, characterized in that: After the pre-treated heterogeneous bonding structure is annealed, the method for manufacturing the heterogeneous bonding structure further includes: The first substrate and the second substrate are thinned to obtain the heterogeneous bonding structure.

9. The method for manufacturing a heterogeneous bonding structure according to claim 7, characterized in that: When the second substrate is an SOI substrate, the SOI substrate includes a stacked Si layer, a buried oxide layer and a silicon substrate, and the second transition layer is formed on the Si layer, after the pre-treated heterogeneous bonding structure is annealed, the method for manufacturing the heterogeneous bonding structure further includes: The buried oxide layer and the silicon substrate are removed by a method combining wet etching and grinding to expose the Si layer included in the second substrate.

10. The method for manufacturing a heterogeneous bonding structure according to claim 1, characterized in that: Before bonding the first transition layer included in the first structure and the second transition layer included in the second structure, the method for manufacturing the heterogeneous bonding structure further includes: The first structure and the second structure are cleaned separately.

Citation Information