Phase change microcapsule for lithium battery pouring sealant and preparation method of phase change microcapsule
By using aluminum hydroxide, the self-assembly reaction product of inorganic water-soluble aluminum ion salts and ammonia water, to coat the phase change paraffin, forming phase change microcapsules with high thermal conductivity and flame retardancy, solving the problems of flammability and low thermal conductivity in the existing technology. problem, improving the safety and temperature control effect of lithium-ion batteries.
Patent Information
- Application Number
- CN202410756131.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-11
AI Technical Summary
The shell and core materials of existing lithium-ion battery phase change microcapsules are both flammable organic materials, which lead to low thermal conductivity, solid-liquid phase change leakage and combustion risks, making it difficult to effectively control the temperature of lithium-ion batteries.
It uses inorganic water-soluble aluminum ion salts and aluminum hydroxide, the self-assembly reaction product of ammonia water, as the outer flame-retardant wall material, combined with phase change paraffin as the inner core material, and is emulsified with anionic surfactants to form high thermal conductivity and flame retardancy. Phase change microcapsules.
It improves the thermal conductivity and flame retardant properties of phase change microcapsules, reduces the risk of solid-liquid phase change leakage, and enhances the safety and temperature control capabilities of lithium-ion batteries.
Smart Images

Figure CN118763313A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of phase change energy storage materials, in particular to a phase change microcapsule for lithium battery potting glue and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density and long cycle life, and are widely used in electric vehicles, energy storage systems, electronic products and other fields. Temperature has a great influence on the performance of lithium batteries. Studies have shown that lithium-ion batteries perform best in the temperature range of 25 to 45°C. During the charging and discharging process of lithium-ion batteries, complex electrochemical reactions occur inside, and the heat generated causes their temperature to rise. High temperature will cause the battery capacity to decay rapidly and cause internal short circuits. When the battery is in a high temperature state for a long time, the heat will continue to accumulate, and eventually a short circuit will occur inside, which will cause thermal runaway of the battery. Under extreme conditions such as over-discharge, extrusion, and puncture, the temperature of lithium-ion batteries rises rapidly until it exceeds the safety upper limit, resulting in thermal runaway. If the temperature cannot be reduced in time, thermal runaway phenomena such as fire or explosion will occur. How to control the operating temperature of lithium batteries within a safe range is an important part of ensuring the safety of lithium batteries.
[0003] Phase change material (PCM) refers to a material that changes its state and provides latent heat when the temperature remains unchanged. Phase change materials will absorb or release a large amount of latent heat. Phase change heat storage materials can perform passive thermal management on lithium-ion batteries. When the temperature of the lithium-ion battery pack is high, PCM absorbs the heat generated by the battery pack to cool the lithium-ion battery pack and stores the heat at the same time. When the temperature is low, the stored heat can be released through phase change for heat preservation, thus realizing passive thermal management of the lithium-ion battery pack. At present, most of the phase change materials used in phase change microcapsules are organic materials, and the carriers coated thereon are usually organic polymer materials. Both are flammable, and the use of the phase change microcapsules will reduce the fire resistance. For example, two Chinese patents with application numbers 201210105056.4 and 201310435991.1 provide a phase change microcapsule composed of acrylic resin as the capsule wall and organic phase change materials such as paraffin as the capsule core. The capsule wall and capsule core of the phase change microcapsule are both flammable organic materials.
[0004] On the other hand, the use of paraffin as a phase change material for lithium-ion batteries requires solving three problems in actual application: first, preventing the leakage of paraffin after solid-liquid phase change; second, improving the thermal conductivity of PCM materials to better exert its temperature control effect; third, improving the flame retardancy of PCM to avoid fire risks such as combustion during use. The existing phase change microcapsule core material is paraffin, and the outer wall material is organic matter, which is easy to burn and has a low thermal conductivity. Summary of the invention
[0005] In order to solve the above problems, the purpose of the present invention is to provide a phase change microcapsule for lithium battery potting glue and a preparation method thereof.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] A phase-change microcapsule for lithium battery potting glue consists of an inner core material and an outer flame-retardant wall material, an emulsifier is distributed between the inner core material and the outer flame-retardant wall material, the inner core material is phase-change paraffin, the outer flame-retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant.
[0008] Preferably, the inorganic water-soluble aluminum ion salt is at least one of aluminum chloride, aluminum sulfate or aluminum nitrate.
[0009] Preferably, the mass ratio of the inner core material to the outer flame-retardant wall material is 1 to 3:1, and the ratio of the inner core material to the emulsifier is 1:0.02 to 0.08.
[0010] Preferably, the anionic surfactant is one or two of A-102, A-103, sodium petroleum sulfonate or sodium secondary alkyl sulfate.
[0011] The present invention also includes a method for preparing phase change microcapsules for lithium battery potting glue, comprising the following steps:
[0012] ① In parts by weight, add 75-85 parts of deionized water into a reaction kettle, add 9-12 parts of paraffin into the reaction kettle while stirring, heat to 60-65°C to melt, add 0.4-0.8 parts of anionic surfactant, stir for 25-30 minutes to form an oil-in-water emulsion;
[0013] ② Dissolve 5 to 33 parts of an inorganic water-soluble aluminum ion salt in 75 to 85 parts of deionized water to obtain an aluminum salt aqueous solution, add it dropwise to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue stirring for 30 minutes to 1 hour after the addition is completed, add 40 to 50 parts of ammonia water to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue reacting for 1 to 2 hours after the addition is completed, and obtain a reaction solution;
[0014] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 35-40° C. for 40-48 hours to obtain phase change microcapsules for lithium battery potting glue.
[0015] Preferably, the mass concentration of the ammonia water is 1 to 3 mol / L.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] The phase change microcapsules for lithium battery potting adhesive of the present invention are obtained by coating paraffin with self-assembled aluminum hydroxide, and have higher thermal conductivity than existing organic shells. Since aluminum hydroxide is an excellent inorganic flame retardant, the problems of low thermal conductivity when phase change materials are added alone, easy leakage and flammability during solid-liquid phase change are solved. The microcapsules are added to lithium ion battery potting adhesive as a phase change filler to improve the safety of lithium ion batteries.
[0018] The preparation method of the phase change microcapsule for lithium battery potting glue of the present invention is ingeniously designed. First, hydrophobic phase change material paraffin is dispersed in water under the action of an anionic emulsifier to form an oil-in-water emulsion; one end of the lipophilic molecular alkyl faces the paraffin, and the negatively charged hydrophilic end faces the water molecule. After the positively charged aluminum ion is added, the positively charged aluminum ion is adsorbed on the surface of the negatively charged emulsifier through the self-assembly effect of positive and negative charges. After ammonia water is dripped, the ionized hydroxide reacts with the aluminum ion on the surface of the emulsifier to form aluminum hydroxide precipitation, and the phase change material paraffin is coated therein to form a flame retardant phase change microcapsule with the flame retardant aluminum hydroxide as the capsule wall and the phase change material paraffin as the core material. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The schematic diagram of the preparation process of the phase change microcapsules for lithium battery potting glue of the present invention;
[0020] Figure 2 It is a schematic diagram of the powder state of the phase change microcapsules for lithium battery potting glue of the present invention. DETAILED DESCRIPTION
[0021] The purpose of the present invention is to provide a phase change microcapsule for lithium battery potting glue and a preparation method thereof, which is achieved by the following technical scheme:
[0022] A phase-change microcapsule for lithium battery potting glue consists of an inner core material and an outer flame-retardant wall material, an emulsifier is distributed between the inner core material and the outer flame-retardant wall material, the inner core material is phase-change paraffin, the outer flame-retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant.
[0023] Preferably, the inorganic water-soluble aluminum ion salt is at least one of aluminum chloride, aluminum sulfate or aluminum nitrate.
[0024] Preferably, the mass ratio of the inner core material to the outer flame-retardant wall material is 1 to 3:1, and the ratio of the inner core material to the emulsifier is 1:0.02 to 0.08.
[0025] Preferably, the anionic surfactant is one or two of A-102, A-103, sodium petroleum sulfonate or sodium secondary alkyl sulfate.
[0026] The present invention also includes a method for preparing phase change microcapsules for lithium battery potting glue, such as Figure 1 As shown, the following steps are included:
[0027] ① In parts by weight, add 75-85 parts of deionized water into a reaction kettle, add 9-12 parts of paraffin into the reaction kettle while stirring, heat to 60-65°C to melt, add 0.4-0.8 parts of anionic surfactant, stir for 25-30 minutes to form an oil-in-water emulsion;
[0028] ② Dissolve 5 to 33 parts of an inorganic water-soluble aluminum ion salt in 75 to 85 parts of deionized water to obtain an aluminum salt aqueous solution, add it dropwise to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue stirring for 30 minutes to 1 hour after the addition is completed, add 40 to 50 parts of ammonia water to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue reacting for 1 to 2 hours after the addition is completed, and obtain a reaction solution;
[0029] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 35-40°C for 40-48 hours to obtain phase change microcapsules for lithium battery potting glue, the powder state is as follows Figure 2 shown.
[0030] Preferably, the mass concentration of the ammonia water is 1 to 3 mol / L.
[0031] The present invention is further described below in conjunction with specific embodiments.
[0032] Example 1
[0033] A phase change microcapsule for lithium battery potting glue, composed of an inner core material and an outer flame retardant wall material, an emulsifier is distributed between the inner core material and the outer flame retardant wall material, the inner core material is phase change paraffin, the outer flame retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant A-102.
[0034] Example 2
[0035] A phase-change microcapsule for lithium battery potting glue, composed of an inner core material and an outer flame-retardant wall material, an emulsifier is distributed between the inner core material and the outer flame-retardant wall material, the inner core material is phase-change paraffin, the outer flame-retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant A-103.
[0036] Example 3
[0037] A phase change microcapsule for lithium battery potting glue consists of an inner core material and an outer flame retardant wall material, an emulsifier is distributed between the inner core material and the outer flame retardant wall material, the inner core material is phase change paraffin, the outer flame retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant sodium petroleum sulfonate.
[0038] Example 4
[0039] A phase-change microcapsule for lithium battery potting glue consists of an inner core material and an outer flame-retardant wall material, an emulsifier is distributed between the inner core material and the outer flame-retardant wall material, the inner core material is phase-change paraffin, the outer flame-retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant sodium secondary alkyl sulfate.
[0040] Example 5
[0041] A phase-change microcapsule for lithium battery potting glue consists of an inner core material and an outer flame-retardant wall material, an emulsifier is distributed between the inner core material and the outer flame-retardant wall material, the inner core material is phase-change paraffin, the outer flame-retardant wall material is aluminum hydroxide, a self-assembly reaction product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant sodium secondary alkyl sulfate and A-102.
[0042] Example 6
[0043] A method for preparing phase change microcapsules for lithium battery potting glue comprises the following steps:
[0044] ① Add 75g of deionized water to the reactor, add 9g of paraffin to the reactor while stirring, heat to 60°C to melt, add 0.4g of anionic surfactant A-102, stir for 25 minutes to form an oil-in-water emulsion;
[0045] ② Dissolve 5g of aluminum nitrate in 75g of deionized water to obtain an aluminum salt aqueous solution, and add it dropwise to the reactor at a rate of 5 drops / 10 seconds. Continue stirring for 30 minutes after the addition is complete. Add 40g of ammonia water with a mass concentration of 3mol / L to the reactor at a rate of 5 drops / 10 seconds. After the addition is complete, continue the reaction for 1 hour to obtain a reaction solution;
[0046] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 35° C. for 40 hours to obtain phase change microcapsules for lithium battery potting glue.
[0047] Example 7
[0048] A method for preparing phase change microcapsules for lithium battery potting glue comprises the following steps:
[0049] ① Add 85g of deionized water to the reactor, add 12g of paraffin to the reactor while stirring, heat to 65°C to melt, add 0.8g of anionic surfactant A-103, stir for 30 minutes to form an oil-in-water emulsion;
[0050] ② Dissolve 33g of aluminum sulfate in 85g of deionized water to obtain an aluminum salt aqueous solution, add it dropwise to the reactor at a rate of 1 drop / second, continue stirring for 1 hour after the addition is complete, add 50g of ammonia water with a mass concentration of 1mol / L to the reactor at a rate of 1 drop / second, continue reacting for 2 hours after the addition is complete, and obtain a reaction solution;
[0051] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 40° C. for 48 hours to obtain phase change microcapsules for lithium battery potting glue.
[0052] Example 8
[0053] A method for preparing phase change microcapsules for lithium battery potting glue comprises the following steps:
[0054] ① Add 78g of deionized water to the reactor, add 10g of paraffin to the reactor while stirring, heat to 62°C to melt, add 0.5g of anionic surfactant sodium petroleum sulfonate, stir for 28 minutes to form an oil-in-water emulsion;
[0055] ② Dissolve 30g of aluminum chloride in 82g of deionized water to obtain an aluminum salt aqueous solution, and add it dropwise to the reactor at a rate of 6 drops / 10 seconds. After the addition is completed, continue stirring for 40 minutes. Add 42g of ammonia water with a mass concentration of 1.5mol / L to the reactor at a rate of 8 drops / 10 seconds. After the addition is completed, continue the reaction for 1.5 hours to obtain a reaction solution;
[0056] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 36° C. for 42 hours to obtain phase change microcapsules for lithium battery potting glue.
[0057] Example 9
[0058] The method for preparing the phase change microcapsules for lithium battery potting glue described in Example 4 comprises the following steps:
[0059] ① Add 82g of deionized water to the reactor, add 11g of paraffin to the reactor under stirring, heat to 62°C to melt, add 0.7g of anionic surfactant sodium secondary alkyl sulfate, stir for 26 minutes to form an oil-in-water emulsion;
[0060] ② Dissolve 25g of aluminum sulfate and 5g of aluminum chloride in 78g of deionized water to obtain an aluminum salt aqueous solution, and add it dropwise to the reactor at a rate of 8 drops / 10 seconds. After the addition is completed, continue stirring for 50 minutes. Add 48g of ammonia water with a mass concentration of 2.5mol / L to the reactor at a rate of 7 drops / 10 seconds. After the addition is completed, continue the reaction for 1.5 hours to obtain a reaction solution;
[0061] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 38° C. for 46 hours to obtain phase change microcapsules for lithium battery potting glue.
[0062] Example 10
[0063] A method for preparing phase change microcapsules for lithium battery potting glue comprises the following steps:
[0064] ① Add 80g of deionized water to the reactor, add 10g of paraffin to the reactor under stirring, heat to 62°C to melt, add 0.2g of secondary alkyl sodium sulfate and 0.3g of anionic surfactant A-102, stir for 28 minutes to form an oil-in-water emulsion;
[0065] ② Dissolve 28g of aluminum nitrate in 80g of deionized water to obtain an aluminum salt aqueous solution, and add it dropwise to the reactor at a rate of 8 drops / 10 seconds. After the addition is completed, continue stirring for 45 minutes. Add 45g of 2mol / L ammonia water to the reactor at a rate of 8 drops / 10 seconds. After the addition is completed, continue the reaction for 1.5 hours to obtain a reaction solution;
[0066] ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 36° C. for 45 hours to obtain phase change microcapsules for lithium battery potting glue.
[0067] During the preparation process, excess water-soluble aluminum salt can be removed by washing with deionized water. The mass ratio of the inner core material (paraffin) and the outer flame-retardant wall material (aluminum hydroxide) of the phase change microcapsule for lithium battery potting glue obtained in the embodiment of the present invention is 1 to 3:1, and the ratio of the inner core material to the emulsifier is 1:0.02 to 0.08.
[0068] Comparative Example 1
[0069] The core material prepared by the method of Example 3 in CN105112020A is fatty acid ester, and the flame retardant wall material is a phase change microcapsule composed of a reactive phosphonate monomer and a pentaerythritol tetraacrylate cross-linked polymer.
[0070] Comparative Example 2
[0071] The flame-retardant phase-change microcapsules were prepared by referring to the method of Example 5 in Chinese patent CN108948076A.
[0072] The phase change microcapsules for lithium battery potting adhesive obtained in Examples 5 to 10 and the microcapsules obtained in Comparative Examples 1 and 2 were tested for thermal conductivity, oxygen index, phase change enthalpy and other properties. The results are shown in Table 1.
[0073] The thermal conductivity is determined by the guarded hot plate method, using GB / T10294-2008 "Guarded hot plate method for determination of steady-state thermal resistance and related properties of thermal insulation materials"
[0074] The average test heat release rate and peak heat release were obtained by cone calorimetry test. The test used a cone calorimeter from FireTest Technology, UK. The ISO 5660-1 standard was selected. 10g of microcapsules were mixed with 11.40g of epoxy resin and cured. The sample size was 100mm×100mm×10mm.
[0075] The limiting oxygen index test was performed using an Atlas Limiting Oxygen Index instrument, with liquefied petroleum gas as the ignition source. 10 g of microcapsules were mixed with 40 g of epoxy resin and cured. The sample size was 125 mm × 10 mm × 4 mm.
[0076] Differential Scanning Calorimeter (DSC): The phase change temperature and phase change enthalpy of the phase change microcapsules were tested using a differential scanning calorimeter (DSC-4000) produced by Perkin-Elmer. About 5 mg of the microcapsule sample was heated from 5°C to 80°C at a heating rate of 10°C / min under nitrogen protection, and then cooled from 80°C to 5°C at a cooling rate of 10°C / min.
[0077] Table 1 Microcapsule performance test results
[0078]
[0079] It can be seen from the results in Table 1 that the phase change microcapsules obtained in the present invention have higher phase change enthalpy, lower heat release rate, higher thermal conductivity, and excellent flame retardant properties than the phase change microcapsules of Comparative Documents 1 and 2.
[0080] By building a lithium-ion battery platform, the charging and discharging of lithium-ion single cells at different ambient temperatures were tested, and the phase-change microcapsules obtained in Example 10 of the present invention were used to cool the battery module, and the heat transfer effect at different ambient temperatures was tested, and compared with the phase-change microcapsules prepared by the method of Example 3 in Comparative Example 1 CN105112020A. The results are shown in Table 2.
[0081] Test process: Use the built experimental platform to conduct charge and discharge tests on lithium-ion batteries. The battery charging system is constant current and constant voltage charging first, and then charging to 100% SOC. The discharge system is constant current discharge. The specific test steps are:
[0082] (1) Place the battery in a thermostat and place it at a test temperature of 5°C;
[0083] (2) When the battery temperature reaches the set ambient temperature, constant current charging is performed at 0.5C. When the voltage reaches 4.25V, constant voltage charging is switched to stop charging when the charging current drops to 0.05C. The battery is left standing for 30 minutes.
[0084] (3) After the battery has been left to rest, discharge it at a constant current of 0.5C until the battery voltage drops to 3V, then stop discharging and leave it to rest for 30 minutes.
[0085] (4) Repeat steps (1), (2), (3) three times.
[0086] (5) Repeat steps (1)(2)(3)(4) to discharge the battery to 3 V at 1C and 1.5C respectively. After all discharges are completed, let it stand for 30 minutes.
[0087] (6) Set the ambient temperature to 25℃ and 40℃, and repeat steps (1)(2)(3)(4)(5).
[0088] Table 2 Maximum battery temperature difference at different ambient temperatures
[0089]
[0090] Compared with the phase change microcapsules without adding phase change microcapsules and the phase change microcapsules of comparative example 1, the phase change microcapsules obtained by the present invention have a smaller temperature difference when working at different ambient temperatures. This is because the phase change microcapsules with aluminum hydroxide as the outer shell have a higher thermal conductivity. When the temperature reaches the melting point of the phase change material, the paraffin in the phase change material will absorb a large amount of heat and transfer heat to the outside, so that the temperature of the lithium battery is maintained in a good working range.
Claims
1. A phase change microcapsule for lithium battery potting glue, Features: It consists of an inner core material and an outer flame retardant wall material, between which an emulsifier is distributed. The inner core material is phase-change paraffin, the outer flame retardant wall material is aluminum hydroxide, a self-assembly product of an inorganic water-soluble aluminum ion salt and ammonia water, and the emulsifier is an anionic surfactant.
2. The phase change microcapsule for lithium battery potting glue according to claim 1, Features: The inorganic water-soluble aluminum ion salt is at least one of aluminum chloride, aluminum sulfate or aluminum nitrate.
3. The phase change microcapsule for lithium battery potting glue according to claim 1, Features: The mass ratio of the inner core material to the outer flame-retardant wall material is 1 to 3:1, and the ratio of the inner core material to the emulsifier is 1:0.02 to 0.
08.
4. The phase change microcapsule for lithium battery potting glue according to claim 1, Features: The anionic surfactant is one or two of A-102, A-103, sodium petroleum sulfonate or sodium secondary alkyl sulfate.
5. A method for preparing a phase change microcapsule for lithium battery potting glue according to claim 1, Features: The following steps are involved: ① In parts by weight, add 75-85 parts of deionized water into a reaction kettle, add 9-12 parts of paraffin into the reaction kettle while stirring, heat to 60-65°C to melt, add 0.4-0.8 parts of anionic surfactant, stir for 25-30 minutes to form an oil-in-water emulsion; ② Dissolve 5 to 33 parts of an inorganic water-soluble aluminum ion salt in 75 to 85 parts of deionized water to obtain an aluminum salt aqueous solution, add it dropwise to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue stirring for 30 minutes to 1 hour after the addition is completed, add 40 to 50 parts of ammonia water to the reaction kettle at a rate of 5 to 10 drops / 10 seconds, continue reacting for 1 to 2 hours after the addition is completed, and obtain a reaction solution; ③ Filter the reaction solution obtained in step ② to obtain a filter cake, rinse it with deionized water to remove the uncoated phase change material, and then dry the filter cake in an oven at 35-40° C. for 40-48 hours to obtain phase change microcapsules for lithium battery potting glue.
6. The phase change microcapsule for lithium battery potting glue according to claim 5, Features: The mass concentration of the ammonia water is 1-3 mol / L.
Citation Information
Cited By
Lithium secondary battery containing flame-retardant microcapsule and preparation method of lithium secondary battery
CN121288238A