Composite coating diaphragm of metal lithium battery, preparation method of composite coating diaphragm and corresponding lithium battery
By setting a solid electrolyte and a lithiophilic oxide paired coating on the lithium battery separator, the growth of lithium dendrites is suppressed, the safety and fast charging performance problems caused by lithium dendrites in lithium batteries are solved, and more efficient lithium ion conduction is achieved. and battery safety.
Patent Information
- Application Number
- CN202410841247.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-31
- Publication Date
- 2024-10-11
AI Technical Summary
The growth of lithium dendrites in metallic lithium batteries leads to uneven deposition, which can easily pierce the separator, causing short circuits and combustion explosions. The fast charging performance is poor, and the existing technology is complex and costly.
Setting specific pairs of coatings on the separator, including solid electrolyte coatings and lithiophilic oxide coatings, inhibits the growth of lithium dendrites by reacting with lithium dendrites and forming lithium alloys, and strengthens the composite coating through multi-layer stacked coating design effect.
It effectively inhibits the growth of lithium dendrites, improves battery safety and fast charging performance, reduces operating and production costs, and improves the electrochemical performance of lithium batteries.
Smart Images

Figure BDA0004914798090000121 
Figure BDA0004914798090000131
Abstract
Description
[0001] This case is a divisional application of a case with an application date of December 31, 2021, an invention name of composite coated diaphragm for metal lithium batteries, preparation method thereof and corresponding lithium battery, and application number CN202111680978.3. Technical Field
[0002] The present invention relates to the field of metal lithium batteries, and in particular to a composite coating diaphragm for metal lithium batteries, a method for preparing the composite coating diaphragm, and a metal lithium battery comprising the composite coating diaphragm. Background Art
[0003] As a type of electrochemical energy storage device, lithium batteries have the advantages of no memory effect, high energy density and long cycle life, and are widely used in many fields, such as portable electronic devices and electric vehicles. Among them, lithium metal has a high theoretical energy density and low electrochemical potential, which improves the overall energy density of the battery. At the same time, it also brings a series of core problems due to its ultra-high chemical reaction activity and uneven lithium deposition. Specifically, the high chemical reaction activity causes metallic lithium to easily react with the electrolyte, resulting in the consumption of the electrolyte; the uneven lithium deposition will lead to the formation of lithium dendrites, which can easily pierce the diaphragm and cause a short circuit, and the dendrites will detach from the roots during lithium removal, forming "dead lithium", causing irreversible capacity loss. Due to the characteristics of lithium deposition, metal lithium batteries have poor kinetic performance, especially poor fast charging performance. The fast charging process is particularly prone to the generation of lithium dendrites, which hinders the practical application of metal lithium batteries.
[0004] Nowadays, many studies focus on solving the problem of lithium dendrite growth. For example, it has been reported that inorganic lithium ion conductors and lithium salts are coated on the diaphragm to induce uniform distribution of lithium ions during lithium deposition (see, for example, CN108365152 B, CN 108695473 A, CN 107819097 A, CN 108777282A, etc.). In addition, another method uses in-situ generation of uniformly dispersed lithium alloys and / or lithium nitride on the surface of the lithium negative electrode to enhance the lithium-philic sites, improve the lithium ion diffusion capacity, and inhibit the generation of lithium dendrites (see, for example, CN 107910496B). However, in the above two methods, once lithium precipitation occurs on the surface of the negative electrode to form dendritic metallic lithium, it may pierce the diaphragm, causing the lithium battery to short-circuit and burn and explode.
[0005] There are also reports that use a composite coating, which first sets a silicon dioxide coating on the surface of the diaphragm substrate, and then sets a boehmite coating on the silicon dioxide coating. Thus, the growth of lithium dendrites is suppressed by SiOx+yLi+ye→Si+LiyOx and yLi+SiOx→LiySiOx (see, for example, CN111211278 A). However, in this method, the theoretical equilibrium potential of the reaction between SiO2 and lithium is low, and it is easy to react with the electrolyte decomposition to produce an organic-based SEI, which is not conducive to the early formation of an inorganic-based SEI containing lithium-philic sites to solve the problem of uneven deposition of metallic lithium. The lithium / electrolyte interface of the former is unstable.
[0006] In addition, there are also solutions such as setting polymer material coatings (such as CN202110308553.3), inorganic and organic composite coatings (such as CN201910707142.4, etc.).
[0007] In addition to the above-mentioned coating method, Xiaoge Hao et al. (“Constructing Multifunctional Interphase between Li 1.4 Al 0.4 Ti 1.6 (PO4)3and Li Metal by Magnetron Sputtering forHighly Stable Solid-State Lithium Metal Batteries”, Advanced Energy Materials, 2019) constructs an ultra-thin ZnO layer on the surface of LATP particles by magnetron sputtering, and reacts with Li in situ to form a solid electrolyte interface phase (SEI) to reduce the interface resistance, inhibit side reactions, and thus inhibit the growth of lithium dendrites. However, the current magnetron sputtering technology is complex and has harsh environmental conditions, which has led to a significant increase in operating and production costs.
[0008] Therefore, it is necessary to find a simple and effective strategy to solve the problems caused by lithium dendrites in metal lithium batteries and further improve the electrochemical performance of lithium batteries. Summary of the invention
[0009] In view of the defects and shortcomings in the prior art, the purpose of the present invention is to provide a composite coating diaphragm for lithium batteries, a preparation method thereof and a corresponding metal lithium battery. The present invention provides a specific paired coating on the diaphragm, so that while homogenizing the lithium ion flow, the growth of lithium dendrites is effectively inhibited, thereby improving the battery safety.
[0010] In a first aspect, the present invention provides a composite separator for a lithium metal battery, comprising:
[0011] Basement membrane;
[0012] a solid electrolyte coating disposed on a base film; and,
[0013] a lithium-philic oxide coating disposed on the solid electrolyte coating,
[0014] The solid electrolyte coating is in the form of a single layer or multiple layers, and contains a solid electrolyte that can react with lithium dendrites; the lithium-philic oxide coating is in the form of a single layer or multiple layers, and contains a lithium-philic oxide that can form a lithium alloy with lithium metal through in-situ electrochemical or chemical reactions.
[0015] In some embodiments, the total thickness of the solid electrolyte coating and the lithium-philic oxide coating is 0.1 μm to 10 μm. The thickness of the solid electrolyte coating is 0.05-5 μm, and the thickness of the lithium-philic oxide coating is 0.05-5 μm.
[0016] In some embodiments, the solid electrolyte capable of reacting with lithium dendrites is selected from one or more of a LIPON-type electrolyte, a NASICON-type electrolyte, a garnet-type electrolyte, a perovskite-type electrolyte, an antiperovskite-type electrolyte, and a LISICON-type electrolyte; in particular, selected from lithium aluminum titanium phosphate Li 1+x Al x Ti 2-x (PO4)3, Lithium Aluminum Germanium Phosphate Li 1+y Al y Ge 2-y (PO4)3, Lithium lanthanum titanium oxide Li z La 2 / 3-z / 3 TiO3, Lithium Lanthanum Zirconium Oxide Li7La3Zr2O 12 and Li 10 GeP2S 12 , Li 10 SnP2S 12 A combination of one or more of <x≤1.5,0<y≤1,0<z≤1.5。
[0017] In some embodiments, the lithium-philic oxide capable of forming a lithium alloy (having a suitable lithium insertion potential) with lithium metal through an in-situ electrochemical or chemical reaction is generally a lithium-philic oxide having a reaction Gibbs free energy of -150 to -350 kJmol- 1 The metal oxide is particularly selected from one or more combinations of zinc oxide, manganous oxide, manganese tetraoxide, ferrous oxide, V2O3, Cr2O3, and Cr3O4.
[0018] In some embodiments, the solid electrolyte coating further includes a dispersant, a thickener, a binder and a wetting agent, and the preferred mass ratio of the solid electrolyte to the dispersant, the thickener, the binder and the wetting agent is 100:(0.3-0.8):(1-9):(3-10):(0.4-1.2); and / or the lithium-philic oxide coating further includes a dispersant, a thickener, a binder and a wetting agent, and the preferred mass ratio of the lithium-philic oxide to the dispersant, the thickener, the binder and the wetting agent is 100:(0.3-0.8):(1-9):(3-10):(0.4-1.2).
[0019] In some embodiments, the binder used can be selected from one or more of polyacrylate, styrene-butadiene rubber, styrene-acrylic emulsion, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polyvinyl acetate, polyurethane, polyethyleneimine, but the present invention is not limited thereto.
[0020] In some embodiments, the thickener used may be selected from one or more of carboxyethyl cellulose, sodium carboxymethyl cellulose, polyacrylamide, and sodium alginate, but the present invention is not limited thereto.
[0021] In some embodiments, the wetting agent used can be selected from one or more of sodium perfluorooctanoate, nonylphenol polyoxyethylene ether, chloroalkyl methoxy alcohol ether, polyoxyethylene alkylamine, sodium butyl tea sulfonate, sodium aryl naphthalene sulfonate, sodium dodecylbenzene sulfonate or sodium alkyl sulfate, but the present invention is not limited thereto.
[0022] In some embodiments, the dispersant used may be selected from one or more of polyethylene glycol, polyacrylic acid, and sodium polyacrylate, but the present invention is not limited thereto.
[0023] In some embodiments, the solid electrolyte coating is in the form of multiple layers, and the lithium-affinity oxide coating is in the form of multiple layers, wherein the solid electrolyte coating and the lithium-affinity oxide have the same number of layers and are arranged alternately. By designing a multi-layer stacking scheme, the effect of the composite coating in suppressing lithium dendrites and accelerating lithium ion conduction can be enhanced. For example, the first solid electrolyte coating placed on the base film is designed with a solid electrolyte that reacts to a greater degree with lithium dendrites, the first lithium-affinity oxide coating placed on the first solid electrolyte coating is used in conjunction with a lithium-affinity oxide with a lower degree of lithium-affinity, the second solid electrolyte coating placed on the first lithium-affinity oxide coating uses a solid electrolyte with a higher ion conductivity, and the second lithium-affinity oxide coating placed on the second solid electrolyte coating uses a lithium-affinity oxide with a higher degree of lithium-affinity. In some embodiments, solid electrolyte coatings and lithium-affinity oxide coatings are provided on both sides of the base film.
[0024] Furthermore, the multi-layer coating design can control the thickness of each layer to enhance the synergistic effect. For example, the thickness decreases from the first solid electrolyte coating to the second lithium-philic oxide coating, thereby forming an interface that is lithium-philic and has strong lithium conductivity in contact with metallic lithium, while the interface close to the base film can effectively eliminate the effect of lithium dendrites. This design can also induce lithium ions to diffuse and deposit to the metallic lithium interface.
[0025] In a second aspect, the present invention provides a method for preparing a composite coating separator for a lithium battery. The method comprises:
[0026] The solid electrolyte capable of reacting with lithium dendrites is mixed and stirred with an optional thickener, a binder, a wetting agent, a dispersant and a solvent, and sand-milled and dispersed to obtain a solid electrolyte coating slurry;
[0027] Mixing a lithium-philic oxide capable of forming a lithium alloy with lithium metal by in-situ electrochemical or chemical means with an optional thickener, a binder, a wetting agent, a dispersant and a solvent, and performing sand milling and dispersion to obtain a lithium-philic oxide coating slurry; and
[0028] Taking the solid electrolyte coating slurry to coat the surface of the base film, and drying it to obtain a solid electrolyte coating; and
[0029] The lithium-philic oxide coating slurry is coated on the solid electrolyte coating and dried to obtain a composite coating diaphragm.
[0030] In some embodiments, the total thickness of the obtained coating is 0.1-10 μm, preferably 1-5 μm, wherein the thickness of the first layer is 0.05-5 μm, and the thickness of the second layer is 0.05-5 μm.
[0031] In some embodiments, the coating is performed using a micro-gravure coating machine.
[0032] In some embodiments, the drying is performed after micro-gravure coating using a coater, and drying is performed while coating, thereby improving production efficiency.
[0033] In some embodiments, the sand milling dispersion is to use a sand mill for 0 to 10 hours to sand mill the raw materials to an average particle size of 0.05 to 1 μm.
[0034] In some embodiments, the solvent used can be selected from one or more of water, ethanol, DMAC, DMF, NMP, and acetonitrile, but the present invention is not limited thereto.
[0035] In a third aspect, the present invention provides a metal lithium battery, comprising the composite coating diaphragm described above or the composite coating diaphragm prepared according to the method described above.
[0036] In the metal lithium battery according to the present invention, a fluorine-containing electrolyte can be used in particular, wherein the solvent contains fluorine, so that the metal lithium battery has an excellent safe and fast charging effect. The fluorine-containing electrolyte components include but are not limited to common fluorinated solvents such as fluoroethylene carbonate (FEC), methyl trifluoroethyl carbonate, ethyl trifluoroethyl carbonate, hydrofluoroether (HFE), fluorinated 1,6-dimethoxyhexane, fluorinated 1,4-dimethoxybutane, and also include but are not limited to common lithium salts such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium difluorooxalatoborate (LiDFOB), lithium difluorophosphate, and other additives, including but not limited to lithium bis(oxalatoborate) (LiBOB).
[0037] In the present invention, by setting specific paired coatings, the conventional complex procedures and harsh environmental conditions for modifying lithium metal negative electrodes are avoided. In addition, the first coating of the present invention includes a solid electrolyte that can react with lithium dendrites, which on the one hand curbs the growth of lithium dendrites, and on the other hand helps to transfer lithium ions and homogenize the lithium ion flow. The second coating of the present invention uses a lithium-philic oxide with a suitable lithium insertion potential that can form a lithium alloy through in-situ electrochemical or chemical reactions to form a stable electrode / electrolyte interface dominated by inorganic components. By stacking the second coating on the first coating, the reaction of the solid electrolyte with the lithium negative electrode before the appearance of lithium dendrites is avoided.
[0038] Therefore, the double-layer design of the present invention plays a synergistic role. Without a suitable lithium-philic oxide, it is impossible to construct a stable electrode / electrolyte interface dominated by inorganic components. Without a suitable inorganic solid electrolyte containing variable-valence transition metal elements, it is impossible to improve the lithium ion conductivity in the direction parallel to the electrode while eliminating lithium dendrites, thereby realizing the island deposition of metallic lithium on the surface of the electrode. For lithium-philic oxides, if the lithium-philic degree is too large (such as the Gibbs free energy of reaction between oxide and lithium <-350kJ / mol), it is not conducive to the lithium ion conduction in the plane direction of the electrode. If the lithium-philic degree is too small (such as the Gibbs free energy of reaction between oxide and lithium >-150kJ / mol), the lithium dendrites are easy to overflow the lithium-philic layer. At this time, if the inorganic solid electrolyte reacts excessively with the lithium dendrites (such as Li 0.5 La 0.5 Ti in TiO3 4+ High content and all converted into Ti 0 ), it is not conducive to the lithium ion conduction in the plane direction of the electrode. If the inorganic solid electrolyte reacts too little with the lithium dendrite (such as Li7La3Zr2O 12 Medium Zr 4+ The content is low and not easily reduced by lithium), which is not conducive to the elimination of lithium dendrites; the overlay coating design significantly improves the electrolyte wettability of the composite diaphragm.
[0039] In the present invention, the metal lithium battery includes a battery whose negative electrode is pure metal lithium and a battery whose negative electrode is a lithium alloy. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0041] The composite coating diaphragm provided by the present invention can be a double-layer coating diaphragm, wherein the second coating layer away from the base film is a lithium-philic oxide with a suitable lithium insertion theoretical equilibrium potential (such as about 1.0-1.5V higher than the theoretical potential of lithium deposition) that can form a lithium alloy through in-situ electrochemical or chemical reactions, producing a stable electrode / electrolyte interface mainly composed of inorganic components, homogenizing lithium deposition, and effectively avoiding the deposition of metallic lithium in the form of dendrites; and the first coating layer close to the base film is a solid electrolyte that reacts with lithium dendrites. On the one hand, the solid electrolyte has high ionic conductivity, which is conducive to lithium ion transfer and homogenizing lithium ion flow; on the other hand, once lithium dendrites appear and pass through the second coating layer of the diaphragm, they will react with them to inhibit the further growth of lithium dendrites, thereby improving battery safety.
[0042] The method for preparing a composite coating diaphragm provided by the present invention mainly comprises the following steps: step 1, mixing an inorganic solid electrolyte, a thickener, a binder, a wetting agent, a dispersant and a solvent, and performing sand grinding and dispersion to obtain a first coating slurry; step 2, mixing a lithium-philic oxide, a thickener, a binder, a wetting agent, a dispersant and a solvent, and performing sand grinding and dispersion to obtain a second coating slurry; step 3, applying the first coating slurry on the surface of a base film, and drying; step 4, coating the second coating slurry on the first coating, and drying to obtain a composite coating diaphragm.
[0043] In the present invention, the base film may be one or more of polyethylene film, polypropylene film, polyethylene / polypropylene double-layer film, polyethylene / polypropylene / polyethylene three-layer film, polypropylene / polyethylene / polypropylene three-layer film, polyimide, glass cellulose separator, non-woven fabric film, preferably polyethylene film, and the surface of the base film may be coated with high temperature resistant ceramic particles, such as aluminum oxide (Al2O3). However, the present invention is not limited thereto.
[0044] In the present invention, the speed of the sand milling dispersion in step 1 can be 100-2000 r / min, such as 1500 r / min, and the sand milling time is 0-10 h, such as 3 h, etc. The particle size is 0.05-1 μm, such as 600 nm.
[0045] The speed of the sand milling dispersion in step 2 can be 100-2000 r / min, such as 1500 r / min, and the sand milling time can be 0-10 h, such as 3 h, etc. The size of the particles is 0.05-1 μm, such as 400 nm.
[0046] The coating process of step 3 and step 4 can be one or a combination of dip coating, blade coating, spray coating, etc. Preferably, the coating process of step 3 and step 4 can be micro gravure coating.
[0047] The drying in step 3 and step 4 can be done by coating machine drying, for example, the temperature of blast drying is 20° C. to 60° C., for example, 40° C., etc.; the drying time is 1 to 5 minutes, for example, 2 minutes.
[0048] It should be understood that when the coating is in the form of multiple layers, the above corresponding steps are repeated.
[0049] The present invention is further described in detail by several specific examples. In addition, unless otherwise specified, the materials and instruments used in the following examples can be obtained by conventional commercial means.
[0050] Example 1
[0051] Step 1: 100 parts by weight of LATP, i.e. lithium aluminum titanium phosphate Li 1.5 Al 0.5 Ti 1.5 (PO4)3, 0.5 parts by weight of sodium polyacrylate, 2 parts by weight of sodium carboxymethyl cellulose, 5 parts by weight of polyacrylate and 0.6 parts by weight of sodium perfluorooctanoate, and an appropriate amount of water are mixed as a solvent, stirred, and subjected to a sand mill dispersion treatment at 1500 r / min for 3 hours to obtain a first coating slurry with a LATP particle size of about 600 nm.
[0052] Step 2, 100 parts by weight of zinc oxide, 0.5 parts by weight of sodium polyacrylate, 2 parts by weight of sodium carboxymethyl cellulose, 5 parts by weight of polyacrylate and 0.6 parts by weight of sodium perfluorooctanoate, and an appropriate amount of water as a solvent are mixed, stirred, and subjected to sand milling and dispersion treatment at 1500 r / min for 3 hours to obtain a second coating slurry, wherein the zinc oxide particles have a particle size of about 400 nm.
[0053] Step 3, polyethylene with aluminum oxide coating on both sides is selected, and the first coating slurry is coated on the surface of the base film by micro-gravure coating, and then air-dried at 40° C. for 5 minutes;
[0054] Step 4: apply the second coating slurry on the first coating by knife coating, and then perform air drying at 40° C. for 5 minutes to obtain a composite coating diaphragm.
[0055] The lithium battery composite diaphragm prepared by the above method includes a base film and a composite coating; measured by a micrometer,
[0056] The basement membrane thickness is 2+9+2μm;
[0057] The composite coating thickness is 1+1μm;
[0058] The lithium battery composite diaphragm prepared by the above method is used to assemble a lithium battery. The battery structure is LFP||metal lithium soft pack battery, and the composite coating faces the negative electrode side. The lithium battery prepared above is subjected to electrochemical testing, and the electrolyte is EC+EMC(3:7) / LiPF6(1M) / VC(2%). The specific electrochemical performance test results are shown in Table 1
[0059] Example 2
[0060] Except that the battery structure is LCO||metal lithium and the solid electrolyte:lithium-philic oxide particle size ratio is 600nm:500nm, other parameters are the same as in Example 1.
[0061] Example 3
[0062] Except that the battery structure is NCM||metal lithium and the solid electrolyte:lithium-philic oxide particle size ratio is 600nm:600nm, other parameters are the same as in Example 1.
[0063] Example 4
[0064] Except that zinc oxide is replaced by MnO and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0065] Example 5
[0066] Except that zinc oxide is replaced by Mn3O4, the battery structure is NCM||metal lithium, and the solid electrolyte:lithium-philic oxide particle size ratio = 600nm:700nm, other parameters are the same as Example 1.
[0067] Example 6
[0068] Except that zinc oxide is replaced by FeO, the battery structure is NCM||metal lithium, and the solid electrolyte:lithium-philic oxide particle size ratio = 600nm:300nm, other parameters are the same as Example 1.
[0069] Example 7
[0070] Except that the lithium-philic oxide zinc oxide is replaced by V2O3, the battery structure is NCM||metal lithium, and the solid electrolyte:lithium-philic oxide particle size ratio = 700nm:400nm, other parameters are the same as Example 1.
[0071] Example 8
[0072] Except that zinc oxide is replaced by Cr2O3, the battery structure is NCM||metal lithium, and the solid electrolyte:lithium-philic oxide particle size ratio = 500nm:400nm, other parameters are the same as Example 1.
[0073] Example 9
[0074] Except that zinc oxide is replaced by Cr3O4 and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0075] Example 10
[0076] In addition to LATP being replaced by LATP and LAGP (Li 1.5 Al 0.5 Ge 1.5 (PO4)3) (mass ratio 1:1), the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0077] Embodiment 11
[0078] In addition to LATP being replaced by LATP and LLTO (Li 0.5 La 0.5 TiO3) (mass ratio 1:1), the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0079] Example 12
[0080] Except that zinc oxide is replaced by a mixture of ZnO and Al2O3 (mass ratio 1:1) and the battery structure is NCM||metal lithium, other parameters are the same as Example 1.
[0081] Embodiment 13
[0082] Except that zinc oxide is replaced by a mixture of ZnO and FeO (mass ratio 1:1) and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0083] Embodiment 14
[0084] Except that the particle size of LATP particles is controlled at 300 nm, the particle size of ZnO particles is controlled at 700 nm, and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0085] Embodiment 15
[0086] Except that the LATP coating thickness is 2 μm, the ZnO coating thickness is 2 μm, and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0087] Example 16
[0088] Except that the composite coating is coated on both sides, the thickness of one side is 1+1 μm, and the battery structure is NCM||metal lithium, other parameters are the same as in Example 1.
[0089] Embodiment 17
[0090] A polyethylene base film without an aluminum oxide coating is used, and the composite coating is designed to have four layers, starting from the layer closest to the base film, which are LLTO, MnO, LATP, and ZnO. The particle size is controlled at 600nm, the thickness of the composite coating is 1+1+1+1μm, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0091] Embodiment 18
[0092] A polyethylene base film without an aluminum oxide coating is used, and the composite coating is designed to be four layers, starting from the closest to the base film, LLTO, MnO, LATP, and ZnO, the particle size is controlled at 600nm, the composite coating thickness is 3+2+1+1μm, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0093] Embodiment 19
[0094] Except that the battery structure is NCM||metal lithium and FEC is used instead of EC in the electrolyte, other parameters are the same as those in Example 1.
[0095] Comparative Example 1
[0096] There is no composite coating, a polyethylene-based film without an aluminum oxide coating is used, and other parameters are the same as in Example 1.
[0097] Comparative Example 2
[0098] There is no composite coating, and a polyethylene-based film with a single-sided 2 μm aluminum oxide coating (the coating faces the negative electrode side) is used. The battery structure is LCO||metal lithium, and other parameters are the same as in Example 1.
[0099] Comparative Example 3
[0100] There is no composite coating, the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0101] Comparative Example 4
[0102] There is no lithium-philic oxide coating, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0103] Comparative Example 5
[0104] There is no lithium-philic oxide coating, the solid electrolyte coating uses LAGP instead of LATP, the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0105] Comparative Example 6
[0106] There is no lithium-philic oxide coating, the solid electrolyte coating uses LLTO instead of LATP, the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0107] Comparative Example 7
[0108] There is no solid electrolyte coating, the battery structure is NCM||metal lithium, and other parameters are the same as Example 1.
[0109] Comparative Example 8
[0110] The lithium-philic oxide ZnO is replaced by AgO, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0111] Comparative Example 9
[0112] The lithium-philic oxide ZnO is replaced by CaO, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0113] Comparative Example 10
[0114] The solid electrolyte component LATP is replaced by LLTO, the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0115] Comparative Example 11
[0116] The solid electrolyte component LATP is replaced by LLZO (Li7La3Zr2O 12 ), the battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0117] Comparative Example 12
[0118] The solid electrolyte coating and the lithium-philic oxide coating are swapped, that is, the lithium-philic oxide coating is close to the base film, and the solid electrolyte coating is close to metallic lithium. The battery structure is NCM||metal lithium, and other parameters are the same as in Example 1.
[0119] Performance Testing
[0120] The 10Ah soft pack batteries assembled with the separators obtained in the above examples and comparative examples were tested. The various parameters of the batteries obtained in the examples and comparative examples were measured according to the test methods known in the art. The results are shown in Table 1 below.
[0121] Table 1. Summary of parameters of the batteries obtained in the examples and comparative examples
[0122]
[0123]
[0124] It can be seen from Table 1 that the double-layer design of the present invention solves the problem of uneven deposition of metallic lithium in the metal lithium battery in the prior art, the precipitation of lithium dendrites, and the large surface area of lithium dendrites, which are easy to react with the electrolyte, resulting in battery gas production and capacity reduction. Furthermore, lithium dendrites may pierce the diaphragm, causing the lithium battery to short-circuit and burn and explode. The electrochemical properties of the diaphragm are improved, thereby enhancing the rate performance of the lithium battery and extending the cycle life of the lithium battery. Compared with the comparative example, Examples 1-19 of the present invention have excellent electrochemical properties. The lithium battery obtained by the present invention can have a capacity retention rate of up to 94% after 50 weeks of 1.5C fast charging cycles, and there is no obvious overcharging phenomenon, that is, there is no obvious dendrite growth.
[0125] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention.
Claims
1. A composite coating diaphragm, comprising: Basement membrane; a solid electrolyte coating disposed on the base film; as well as, a lithium-philic oxide coating disposed on the solid electrolyte coating; The solid electrolyte coating comprises a solid electrolyte capable of reacting with lithium dendrites, The lithium-philic oxide coating comprises a lithium-philic oxide that can react with lithium metal to form a lithium alloy through in-situ electrochemical or chemical reactions, and is selected from metal oxides having a Gibbs free energy of reaction with lithium of -150 to -350 kJ / mol; the thickness of the lithium-philic oxide coating is 0.05 to 5 μm.
2. The composite coating membrane according to claim 1, wherein: The lithium-philic oxide coating is in the form of a single layer or multiple layers, And / or, the thickness of the lithium-philic oxide coating is 0.05-2 μm.
3. The composite coating membrane according to claim 2, wherein: The solid electrolyte capable of reacting with lithium dendrites is selected from one or more of a LIPON electrolyte, a NASICON electrolyte, a garnet electrolyte, a perovskite electrolyte, an antiperovskite electrolyte and a LISICON electrolyte; And / or, the lithium-philic oxide is selected from one or more combinations of zinc oxide, manganous oxide, manganese tetraoxide, ferrous oxide, V2O3, Cr2O3, and Cr3O4.
4. The composite coating diaphragm according to claim 1, wherein: The solid electrolyte that can react with lithium dendrites is selected from lithium aluminum titanium phosphate Li 1+x Al x Ti 2-x (PO4)3, Lithium Aluminum Germanium Phosphate Li 1+ y Al y Ge 2-y (PO4)3, Lithium lanthanum titanium oxide Li z La 2 / 3-z / 3 TiO3, Lithium Lanthanum Zirconium Oxide Li7La3Zr2O 12 and Li 10 GeP2S 12 , Li 10 SnP2S 12 One or more combinations of <x≤1.5,0<y≤1,0<z≤1.5。 5. The composite coating diaphragm according to claim 1, wherein: The solid electrolyte that can react with lithium dendrites is selected from lithium aluminum titanium phosphate Li 1+x Al x Ti 2-x (PO4)3, Lithium Aluminum Germanium Phosphate Li 1+ y Al y Ge 2-y At least one of (PO4)3, wherein 0 <x≤1.5,0<y≤1,0<z≤1.5。 6. The composite coating diaphragm according to claim 1, wherein: At least one of the multiple solid electrolytes capable of reacting with lithium dendrites is selected from lithium aluminum titanium phosphate Li 1+x Al x Ti 2- x (PO4)3, Lithium Aluminum Germanium Phosphate Li 1+y Al y Ge 2-y (PO4)3, where 0 <x≤1.5,0<y≤1,0<z≤1.5。 7. The composite coating diaphragm according to claim 2, wherein: The total thickness of the solid electrolyte coating and the lithium-philic oxide coating is 0.1-10 μm; wherein the thickness of the solid electrolyte coating is 0.05-5 μm.
8. The composite coating membrane according to any one of claims 1 to 7, wherein: The solid electrolyte coating is in the form of multiple layers, and the lithium-philic oxide coating is in the form of multiple layers; the solid electrolyte coating and the lithium-philic oxide have the same number of layers and are arranged alternately.
9. The composite coating diaphragm according to any one of claims 8, wherein: The ionic conductivity of each solid electrolyte coating in the multi-layer solid electrolyte coating increases with the increase of the distance between the layer and the base film. The lithium affinity of each lithium-philic oxide coating in the multi-layer lithium-philic oxide coating increases with the increase of the distance between the layer and the base film.
10. The composite coating diaphragm according to any one of claims 1 to 7, wherein: Both sides of the base membrane are provided with a solid electrolyte coating and a lithium-philic oxide coating.
11. A method for preparing the composite coating separator for lithium battery according to claims 1-10, comprising: The solid electrolyte capable of reacting with lithium dendrites is mixed and stirred with an optional thickener, a binder, a wetting agent, a dispersant and a solvent, and sand-milled and dispersed to obtain a solid electrolyte slurry; The lithium-philic oxide capable of forming a lithium alloy with lithium metal through an in-situ electrochemical or chemical reaction is mixed with an optional thickener, a binder, a wetting agent, a dispersant and a solvent, and sand-milled and dispersed to obtain a lithium-philic oxide slurry; and coating the solid electrolyte slurry on the surface of the base film using a coating machine, and drying to obtain a solid electrolyte coating; The lithium-philic oxide slurry is coated on the solid electrolyte coating and dried to obtain a composite coating diaphragm.
12. The method according to claim 11, wherein: The solid electrolyte capable of reacting with lithium dendrites is selected from one or more of a LIPON electrolyte, a NASICON electrolyte, a garnet electrolyte, a perovskite electrolyte, an antiperovskite electrolyte and a LISICON electrolyte; And / or, the lithium-philic oxide capable of forming a lithium alloy with lithium metal through an in-situ electrochemical or chemical reaction is a metal oxide having a Gibbs free energy of reaction with lithium in the range of -150 to -350 kJ / mol.
13. The method according to claim 12, wherein: The solid electrolyte capable of reacting with lithium dendrites is selected from phosphorus Li 1+x Al x Ti 2-x (PO4)3, Lithium Aluminum Germanium Phosphate Li 1+ y Al y Ge 2-y (PO4)3, Lithium lanthanum titanium oxide Li z La 2 / 3-z / 3 TiO3, Lithium Lanthanum Zirconium Oxide Li7La3Zr2O 12 and Li 10 GeP2S 12 , Li 10 SnP2S 12 One or more combinations of <x≤1.5,0<y≤1,0<z≤1.5; And / or, the lithium-philic oxide is selected from one or more combinations of zinc oxide, manganous oxide, manganese tetraoxide, ferrous oxide, V2O3, Cr2O3, and Cr3O4.
14. A metal lithium battery, comprising the composite coating separator according to any one of claims 1 to 10 or the composite coating separator obtained by the method according to any one of claims 11 to 13.
Citation Information
Patent Citations
Lithium ion battery with diaphragm
CN107819097A
A lithium metal anode for secondary batteries, its preparation method and its application
CN107910496B
A composite separator for lithium batteries
CN108365152B
Lithium ion battery diaphragm and preparation method thereof
CN108695473A
Ceramic coating method of lithium battery diaphragm
CN108777282A
Cited By
Composite solid electrolyte layer and preparation method and application thereof
CN120413839A
Lithium ion battery diaphragm with dual-function coating and preparation method of lithium ion battery diaphragm
CN122026002A