Semiconductor structure and manufacturing method thereof
Through laser processing and epitaxial growth processes, the problem of poor filling of holes in the semiconductor structure is solved, the density and conductivity of the silicon material layer are improved, the yield of the semiconductor structure is improved, and adverse effects on other parts are avoided.
Patent Information
- Application Number
- CN202310312374.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-11
AI Technical Summary
Under high integration density of semiconductor structures, the problem of large hole aspect ratio leads to poor filling of filling materials and affects the structural yield.
Laser processing technology is used to heat the initial silicon material layer to melt it in the blind hole. During the cooling and recrystallization process, the underlying silicon is used as a seed crystal to form a silicon material layer with low defect density. Combined with the epitaxial growth process, the blind hole is An underlying silicon is formed on the bottom to reduce corner roughness.
It improves the density and conductivity of the silicon material layer, avoids the formation of voids and gaps, and improves the yield of the semiconductor structure. At the same time, local heating does not affect the temperature of adjacent structures.
Smart Images

Figure CN118765110A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present disclosure relate to the field of semiconductor technology, and in particular to a semiconductor structure and a method for manufacturing the same. Background Art
[0002] As semiconductor structures develop toward higher integration density, the manufacturing methods of semiconductor structures face greater challenges. For example, due to the shortening of the spacing between adjacent structures, the larger the aspect ratio of the holes formed between adjacent structures, the more likely it is to have an adverse effect on the subsequent filling of the holes with filling materials, which is not conducive to improving the yield of the semiconductor structure. Summary of the invention
[0003] The embodiments of the present disclosure provide a semiconductor structure and a method for manufacturing the same, which are at least beneficial to improving the yield of the semiconductor structure.
[0004] According to some embodiments of the present disclosure, on the one hand, an embodiment of the present disclosure provides a method for manufacturing a semiconductor structure, comprising: providing a substrate, wherein the substrate has at least one blind hole; using an epitaxial growth process to form a bottom layer of silicon at least at the bottom of the blind hole; forming an initial silicon material layer filling the remaining blind holes, wherein the melting point of the initial silicon material layer is lower than the melting point of the bottom layer of silicon; using a laser to process the initial silicon material layer so that the initial silicon material layer melts; and cooling the initial silicon material layer after the laser processing so that the initial silicon material layer recrystallizes to form a silicon material layer.
[0005] In some embodiments, in the step of processing the initial silicon material layer with a laser, voids in the initial silicon material layer are eliminated.
[0006] In some embodiments, the silicon material layer includes at least one of single crystal silicon or polycrystalline silicon, and a defect density of the silicon material layer is lower than a defect density of the initial silicon material layer.
[0007] In some embodiments, the working mode of the laser includes a pulsed laser, and the use of the laser to process the initial silicon material layer includes: sequentially performing N pulsed laser processes on the initial silicon material layer located in the blind hole to achieve local heating of the initial silicon material layer located in the blind hole, wherein N is a positive integer, and as the number of times increases, the energy density of the pulsed laser remains unchanged or increases.
[0008] In some embodiments, the energy density of the pulsed laser is in the range of 0.3 mJ / cm 2 ~0.7mJ / cm 2 The wavelength of the laser pulse is 532 nm, and the pulse width of the laser pulse is 10 ns.
[0009] In some embodiments, as the number of times increases, the energy density of the pulsed laser remains unchanged at first and then gradually increases. When the energy density of the pulsed laser remains unchanged, the initial silicon material layer is preheated, and when the energy density of the pulsed laser increases, the melting of the initial silicon material layer is accelerated.
[0010] In some embodiments, in the step of processing the initial silicon material layer with laser pulses, the maximum temperature of the initial silicon material layer is 1100° C. to 1400° C.
[0011] In some embodiments, in the step of processing the initial silicon material layer with laser pulses, a maximum depth of the melted initial silicon material layer along a depth direction of the blind hole is 400 nm to 500 nm.
[0012] In some embodiments, before forming the bottom silicon layer, the method further includes: cleaning the substrate.
[0013] In some embodiments, in the step of forming a bottom layer of silicon at least at the bottom of the blind hole using an epitaxial growth process, a silicon film layer is formed on the sidewall of the blind hole; the bottom layer of silicon and the silicon film layer together form a contact hole, and the forming of an initial silicon material layer filling the blind hole includes: forming an initial silicon material layer filling the contact hole; in the step of processing the initial silicon material layer using a laser, the silicon film layer also melts; in the step of recrystallizing the initial silicon material layer, the silicon film layer in a molten state and the initial silicon material layer in a molten state recrystallize together.
[0014] In some embodiments, along the depth direction of the blind hole, the thickness of the bottom silicon is in the range of 1 nm to 5 nm.
[0015] In some embodiments, the cooling process includes: blowing an inert gas toward the initial silicon material layer after the laser treatment, and the pressure of the inert gas has a numerical range of 0.2 MPa to 1 MPa.
[0016] In some embodiments, the step of providing the base includes: providing a substrate; forming a plurality of parallel bit lines and a dielectric layer located between adjacent bit lines on the substrate, wherein the dielectric layer and the bit lines together enclose a plurality of blind holes, and the blind holes are capacitor contact holes; or, forming a plurality of grooves for forming bit lines in the substrate, wherein the grooves have the blind holes, and the blind holes are used to form a bit line contact layer.
[0017] According to some embodiments of the present disclosure, on the other hand, a semiconductor structure is provided, comprising: a substrate having at least one blind hole therein; a silicon material layer located at least at the bottom and part of the side wall of the blind hole, wherein the defect density of the silicon material layer is lower than the defect density of amorphous silicon.
[0018] In some embodiments, the base includes: a substrate; a plurality of parallel bit lines located on the substrate and a dielectric layer located between adjacent bit lines, the dielectric layer and the bit lines together enclosing a plurality of blind holes; along the extension direction of the blind holes, the silicon material layer is located in the blind holes at a partial depth.
[0019] The technical solution provided by the embodiments of the present disclosure has at least the following advantages:
[0020] On the one hand, after forming an initial silicon material layer that fills the blind holes, the initial silicon material layer is heated by laser so that the initial silicon material layer is in a molten state in the blind holes, which is beneficial to avoid the presence of voids or gaps in the silicon material layer formed by subsequent cooling and recrystallization of the initial silicon material layer, thereby helping to improve the film uniformity of the silicon material layer itself and avoid the problem of poor conductivity caused by the presence of holes in the silicon material layer.
[0021] On the other hand, before forming the initial silicon material layer that fills the blind hole, a bottom silicon is formed at the bottom of the blind hole. Since the melting point of the initial silicon material layer is lower than the melting point of the bottom silicon, when the initial silicon material layer is subsequently heated by laser, the initial silicon material layer can be heated to a molten state, while the bottom silicon is in a non-molten state, so that in the subsequent cooling and recrystallization process of the molten initial silicon material layer, the molten initial silicon material layer can use the bottom silicon as a seed layer and recrystallize along the crystal direction of the crystal in the bottom silicon, so that the silicon material layer finally formed includes at least one of single crystal silicon or polycrystalline silicon, which is conducive to improving the density of the silicon material layer. It can be understood that the bottom silicon provides a better recrystallization condition for the molten initial silicon material layer, which is conducive to further reducing the defect density of the silicon material layer itself, thereby facilitating the improvement of the yield of the silicon material layer and the semiconductor structure. Moreover, the epitaxial growth process is used to form the bottom silicon at least at the bottom of the blind hole, which is conducive to reducing the roughness of the bottom corner of the blind hole through the bottom silicon, and is conducive to improving the film uniformity of the initial silicon material layer subsequently formed on the basis of the bottom silicon.
[0022] On the other hand, since the laser can achieve the effect of local heating, when the laser generates a relatively high temperature in the initial silicon material layer, the temperature generated in other structures adjacent to the initial silicon material layer is relatively low, that is, the temperature generated by the laser in other structures adjacent to the initial silicon material layer has a relatively small impact; and since the laser can achieve the effect of rapid heating, that is, the high temperature lasts for a relatively short time in the initial silicon material layer, the time of temperature impact on other structures adjacent to the initial silicon material layer is also relatively short. Therefore, even if the initial silicon material layer is placed in a high-temperature molten state by the laser, the temperature impact generated by the laser on other structures adjacent to the initial silicon material layer can be ignored, and will not have an adverse effect on other properties of the semiconductor structure.
[0023] In summary, the manufacturing method of the semiconductor structure provided by one embodiment of the present disclosure improves the density and conductivity of the formed silicon material layer to improve the yield of the semiconductor structure, while avoiding the process of forming the silicon material layer from causing adverse effects on other parts of the semiconductor structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] One or more embodiments are exemplarily illustrated by pictures in the corresponding drawings, which do not constitute a limitation on the embodiments. Elements with the same reference numerals in the drawings are represented as similar elements, and the figures in the drawings do not constitute a scale limitation unless otherwise stated. In order to more clearly illustrate the embodiments of the present disclosure or the technical solutions in the traditional technology, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present disclosure. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 A schematic diagram of a process for manufacturing a semiconductor structure provided by an embodiment of the present disclosure;
[0026] Figures 2 to 14 A schematic structural diagram corresponding to each step of a method for manufacturing a semiconductor structure provided in one embodiment of the present disclosure. DETAILED DESCRIPTION
[0027] As can be seen from the background technology, the yield of semiconductor structures needs to be improved.
[0028] The embodiment of the present disclosure provides a semiconductor structure and a manufacturing method thereof. In the manufacturing method, on the one hand, the initial silicon material layer is heated by laser, which is conducive to avoiding the existence of voids or gaps in the silicon material layer formed by the subsequent melting and recrystallization of the initial silicon material layer, thereby improving the compactness and conductivity of the silicon material layer; on the other hand, before forming the initial silicon material layer, a bottom silicon that can provide better recrystallization conditions for the initial silicon material layer is formed at the bottom of the blind hole, thereby facilitating the formation of a silicon material layer with a lower defect density; on the other hand, since the laser can achieve the effect of local heating and the laser can achieve the effect of rapid heating, when the initial silicon material layer is placed in a high-temperature molten state by laser, the temperature effect of the laser on other structures adjacent to the initial silicon material layer can be ignored, and will not cause adverse effects on other properties of the semiconductor structure. Therefore, the manufacturing method of the semiconductor structure provided by an embodiment of the present disclosure is conducive to avoiding the process of forming the silicon material layer from causing adverse effects on other parts of the semiconductor structure while improving the compactness and conductivity of the silicon material layer formed.
[0029] The following will describe the various embodiments of the present disclosure in detail with reference to the accompanying drawings. However, it will be appreciated by those skilled in the art that in the various embodiments of the present disclosure, many technical details are provided in order to enable the reader to better understand the embodiments of the present disclosure. However, even without these technical details and various changes and modifications based on the following embodiments, the technical solutions claimed in the embodiments of the present disclosure can be implemented.
[0030] An embodiment of the present disclosure provides a method for manufacturing a semiconductor structure. The method for manufacturing a semiconductor structure provided by an embodiment of the present disclosure will be described in detail below with reference to the accompanying drawings. Figure 1 A schematic diagram of a process for manufacturing a semiconductor structure provided by an embodiment of the present disclosure; Figures 2 to 14 The schematic diagram of the structure corresponding to each step of the method for manufacturing a semiconductor structure provided in one embodiment of the present disclosure is shown in FIG. Figures 2 to 14 All of them are schematic diagrams of local structures of semiconductor structures.
[0031] refer to Figures 1 to 14 , a method for manufacturing a semiconductor structure includes the following steps.
[0032] S101: Reference Figures 2 to 6 , providing a substrate 100 having at least one blind hole 110 therein.
[0033] In some embodiments, reference Figure 3 and Figure 4The step of providing the base 100 may include: providing a substrate 101 , forming a plurality of grooves 112 for forming the bit lines 102 in the substrate 101 , wherein the grooves 112 have blind holes 110 , and the blind holes 110 are used to form the bit line contact layers 122 .
[0034] It should be noted that Figure 3 A schematic diagram of a partial top view of a substrate 100 in a manufacturing method provided in an embodiment of the present disclosure is shown in FIG. Figure 4 FIG. 1 schematically shows a groove 112 and a blind hole 110 in a substrate 101 for forming a bit line 102. The bit line 102 is drawn in a perspective manner. Figure 3 The area framed by the middle dotted line is the area where the groove 112 in the substrate 101 is located; Figure 4 for Figure 2 The cross-sectional structure diagram of the substrate 100 along the first cross-sectional direction AA1 is shown.
[0035] In one example, refer to Figure 3 and Figure 4 The bit line 102 includes a plurality of bit line contact layers 122 and a bit line body 132 that is in contact with the plurality of bit line contact layers 122 . The bit line contact layers 122 are located in the blind holes 110 and the bit line contact layers 122 correspond to the blind holes 110 one by one. The bit line body 132 is located on the top surface of the bit line contact layers 122 .
[0036] In other embodiments, reference Figure 5 and Figure 6 The step of providing a base 100 may include: providing a substrate 101; forming a plurality of parallel bit lines 102 and a dielectric layer 103 located between adjacent bit lines 102 on the substrate 101, wherein the dielectric layer 103 and the bit lines 102 together enclose a plurality of blind holes 110, and the blind holes 110 are capacitor contact holes.
[0037] It should be noted that Figure 5 FIG. 1 is another partial cross-sectional structural schematic diagram of a substrate 100 in a manufacturing method provided in an embodiment of the present disclosure. Figure 6 for Figure 5 A schematic top view of the structure of the substrate 100 is shown.
[0038] In some embodiments, reference Figure 5 The bit line 102 includes a bit line contact layer 122, a diffusion barrier layer 142, a bit line conductive layer 152, a first bit line protection layer 162 and a second bit line protection layer 172, wherein one bit line 102 may include multiple bit line contact layers 122, multiple bit line contact layers 122 in one bit line 102 are all in contact with and connected to the same diffusion barrier layer 142, the first bit line protection layer 162 and the second bit line protection layer 172 jointly surround the side wall and top surface of the bit line 102 to achieve insulation between the bit line 102 and other conductive structures.
[0039] In some embodiments, reference Figure 5 , the first bit line protection layer 162 is located in the second bit line protection layer 172. In some embodiments, the material of the first bit line protection layer 162 may be silicon oxide, and the material of the second bit line protection layer 172 may be silicon nitride. In some embodiments, the material of the bit line contact layer 122 may be doped polysilicon, the material of the diffusion barrier layer 142 may be titanium nitride, and the material of the bit line conductive layer 152 may be tungsten.
[0040] Continue to refer Figure 5 , the substrate 101 may include an active region 111, a shallow trench isolation structure 121 and an isolation layer 131, the bit line contact layer 122 is in contact with the active region 111, and the isolation layer 131 is provided between the diffusion barrier layer 142 that is not in contact with the bit line contact layer 122 and the shallow trench isolation structure 121, so as to further ensure the insulation between the bit line 102 except the bit line contact layer 122 and the substrate 101. In some embodiments, the material of the shallow trench isolation structure 121 may be silicon oxide or silicon nitride, and the material of the isolation layer 131 may be silicon oxide.
[0041] Continue to refer Figure 5 The blind hole 110 exposes a portion of the active area 111 and the shallow trench isolation structure 121 .
[0042] It is understood that the capacitor contact hole is subsequently used to form a capacitor contact layer, referring to Figure 6 There are multiple blind holes 110 between adjacent bit lines 102, and one blind hole 110 corresponds to a capacitor contact layer formed subsequently.
[0043] It should be noted that the method for manufacturing a semiconductor structure provided in an embodiment of the present disclosure includes but is not limited to being applied in the above-mentioned various embodiments. It is understandable that in the method for manufacturing a semiconductor structure provided in an embodiment of the present disclosure, the solution of the final ready-made silicon material layer in the blind hole 110 can be applied to any scenario where a silicon material layer needs to be formed in a groove or hole, so as to improve the density and conductivity of the silicon material layer while avoiding the process of forming the silicon material layer from causing adverse effects on other parts of the semiconductor structure.
[0044] S102: Reference Figures 7 to 9 , an epitaxial growth process is used to form a bottom silicon layer 104 at least at the bottom of the blind hole 110.
[0045] It should be noted that Figures 7 to 9 Three embodiments of forming the bottom silicon 104 at the bottom of the blind hole 110 by using an epitaxial growth process are shown, wherein: Figure 8 and Fig. 9The existing blind hole 110 is used as a capacitor contact hole as an example. In practical applications, Figure 8 and Fig. 9 The embodiment of the ready-made bottom silicon 104 is also applicable to the case where the blind hole 110 is used to form the bit line contact layer. In addition, according to the application of the blind hole 110, the bottom silicon 104 can be as follows: Figure 7 As shown, a relatively flat thin layer can also be Figure 8 and Fig. 9 Shown is a thin layer forming a groove.
[0046] In some embodiments, after the blind hole 110 is formed, an epitaxial growth process may be directly used to form the bottom silicon 104 at least at the bottom of the blind hole 110 .
[0047] In other embodiments, before forming the bottom silicon 104, the method for manufacturing the semiconductor structure may further include: cleaning the substrate 100. It is understood that before performing the epitaxial process, the substrate 100 including the blind hole 110 is first cleaned to remove impurities that may remain in the blind hole 110, such as interlayer oxides, hydrogen-containing impurities or water vapor, etc. This is conducive to providing a better growth condition for the epitaxial process, such as forming the bottom silicon 104 with a lower defect density based on the clean bottom of the blind hole 110, and avoiding the impurities remaining in the blind hole 110 from reducing the conductivity of the silicon material layer subsequently formed in the blind hole 110, thereby helping to reduce the contact resistance between the active area 111 and the silicon material layer, so as to improve the device performance of the semiconductor structure.
[0048] It can be understood that the use of an epitaxial growth process to form the underlying silicon 104 is conducive to forming an underlying silicon 104 with high density and stable structure. Moreover, due to the characteristics of the epitaxial growth process, it is conducive to forming a thinner underlying silicon 104, which is conducive to improving the film uniformity of the underlying silicon 104. When the doped ions in the subsequent silicon material layer enter the underlying silicon 104, the thickness of the underlying silicon 104 is thinner, which is more conducive to the diffusion of doped ions into the underlying silicon 104, so as to ensure that the concentration of doped ions in the underlying silicon 104 is high, so as to ensure the good conductivity of the underlying silicon 104.
[0049] In some embodiments, the cleaning process includes plasma cleaning, for example, using plasma containing argon or nitrogen to remove impurities remaining in the blind hole 110 and provide a better growth environment for the subsequent epitaxial growth process.
[0050] In some embodiments, reference Figure 8 or Fig. 9 , in the epitaxial growth process, at least in the blind hole 110 (reference Figure 5), in the step of forming the bottom silicon 104 at the bottom of the blind hole 110, a silicon film layer 114 is formed on the sidewall of the blind hole 110; the bottom silicon 104 and the silicon film layer 114 together surround the contact hole 120.
[0051] In one example, refer to Figure 8 , in the blind hole 110 (reference Figure 5 ), in the step of forming the bottom silicon 104 at the bottom of the blind hole 110, the silicon film layer 114 is formed only on the sidewall of the blind hole 110. Figure 8 , in the blind hole 110 (reference Figure 5 ), in the step of forming the bottom silicon 104 at the bottom of the blind hole 110, a silicon film layer 114 is formed on the sidewalls of the blind hole 110 and the top surface of the bit line 102.
[0052] In the above example, the material of the bottom silicon 104 may be single crystal silicon or densified undoped polycrystalline silicon, and the material of the silicon film layer 114 may be polycrystalline silicon.
[0053] It should be noted that Figure 8 and Fig. 9 In order to distinguish the bottom silicon 104 and the silicon film layer 114, different filling methods are used for the bottom silicon 104 and the silicon film layer 114. It can be understood that the bottom silicon 104 and the silicon film layer 114 can be formed in the same step by an epitaxial growth process, that is, the bottom silicon 104 and the silicon film layer 114 are an integrated structure.
[0054] In the above example, it can be understood that before the initial silicon material layer is formed, a bottom silicon 104 is formed at the bottom of the blind hole 110. In the subsequent cooling and recrystallization process of the molten initial silicon material layer, the molten initial silicon material layer can use the bottom silicon 104 as a seed layer and recrystallize along the crystal orientation of the crystal in the bottom silicon 104, so that the silicon material layer finally formed includes at least one of single crystal silicon or polycrystalline silicon, which is conducive to improving the density of the silicon material layer. Moreover, the bottom silicon 104 provides a better recrystallization condition for the molten initial silicon material layer, which is conducive to further reducing the defect density of the silicon material layer itself, thereby facilitating improving the yield of the silicon material layer and the semiconductor structure. In addition, the epitaxial growth process is used to form the bottom silicon 104 at least at the bottom of the blind hole 110, which is conducive to reducing the roughness of the bottom corner of the blind hole 110 through the bottom silicon 104, and is conducive to improving the film uniformity of the initial silicon material layer subsequently formed on the basis of the bottom silicon 104.
[0055] It can be understood that, during the subsequent melting process of the initial silicon material layer, the laser heating temperature can also be controlled to melt the bottom silicon 104 as well; during the subsequent cooling and recrystallization process of the molten initial silicon material layer, the molten bottom silicon 104 crystallizes earlier than the molten initial silicon material layer, and thus the bottom silicon 104 that has been crystallized first is beneficial for providing better recrystallization conditions for the initial silicon material layer that is still in a molten state, and is beneficial for further reducing the defect density of the silicon material layer itself, thereby being beneficial for improving the yield of the silicon material layer and the semiconductor structure.
[0056] In some embodiments, reference Figures 7 to 9 , along the depth direction Z of the blind hole 110, the thickness D of the bottom silicon 104 ranges from 1nm to 5nm. It can be understood that the formation of the bottom silicon 104 is to serve as a seed layer for the subsequent recrystallization of the melted initial silicon material layer, so the thickness of the bottom silicon 104 does not need to be too thick, and the time required for the epitaxial growth process to form the bottom silicon 104 is long. Therefore, the thickness D of the bottom silicon 104 ranges from 1nm to 5nm, which is beneficial to ensure that the bottom silicon 104 is thin while avoiding the formation of the bottom silicon 104. It is beneficial to improve the yield of the semiconductor structure formed subsequently and improve the preparation efficiency of the semiconductor structure. In addition, if the thickness D of the bottom silicon 104 is too large, for example, greater than 5nm, it is not conducive to the entry of doped ions in the initial silicon material layer into the bottom silicon 104 when the initial silicon material layer is deposited in the next step, which is not conducive to improving the conductive performance of the capacitor contact layer finally formed.
[0057] It should be noted that for the convenience of description, Fig. 9 The example shown is described in the subsequent steps.
[0058] S103: Combined with reference Figure 7 and Fig.10 , or in combination with reference Fig. 9 and Fig.11 , forming an initial silicon material layer 105 filling up the remaining blind holes 110 , wherein the melting point of the initial silicon material layer 105 is lower than the melting point of the underlying silicon 104 .
[0059] In some embodiments, reference Figure 7 and Fig.10 , only the bottom silicon 104 is formed at the bottom of the blind hole 110 , the sidewalls of the blind hole 110 and the top surface of the substrate 100 are exposed, and the formed initial silicon material layer 105 is located on the sidewalls of the blind hole 110 and the top surface of the substrate 100 .
[0060] In other embodiments, reference Fig. 9 and Fig.11 , in the blind hole 110 (reference Figure 5), and a silicon film layer 114 is formed on the sidewall of the blind hole 110, and on the basis that the bottom silicon 104 and the silicon film layer 114 together surround the contact hole 120, the step of forming an initial silicon material layer 105 that fills the blind hole 110 may include: forming an initial silicon material layer 105 that fills the contact hole 120.
[0061] In the above embodiments, reference Fig.10 or Fig.11 , after forming the remaining blind hole 110 (reference Figure 5 ), due to the formation process and the aspect ratio of the remaining blind hole 110, the initial silicon material layer 105 is prone to have voids 115 inside. The voids 115 will reduce the film uniformity of the initial silicon material layer 105 and reduce the conductivity of the initial silicon material layer 105 itself. It can be understood that the voids 115 can be macroscopic holes.
[0062] In some embodiments, the method of forming the initial silicon material layer 105 includes CVD (Chemical Vapor Deposition), and the raw material for forming the initial silicon material layer 105 includes silane.
[0063] In some embodiments, the initial silicon material layer 105 may be polysilicon.
[0064] S104: using laser to process the initial silicon material layer 105 so that the initial silicon material layer 105 melts.
[0065] In some embodiments, reference Fig.10 , the silicon film layer 114 is not formed at the same time as the underlying silicon 104 is formed, and thus in the step of processing the initial silicon material layer 105 with a laser, only the initial silicon material layer 105 is melted.
[0066] In other embodiments, in combination with reference Fig.11 and Fig.12 , in the blind hole 110 (reference Figure 5 ) forms a bottom silicon layer 104 at the bottom, and a silicon film layer 114 is formed on the sidewall of the blind hole 110. In the step of using laser to process the initial silicon material layer 105, the silicon film layer 114 is also melted. It should be noted that Fig.12 In the figure, the initial silicon material layer 105 in a molten state and the silicon film layer 114 in a molten state are uniformly drawn as a layer to be crystallized 106 .
[0067] It can be understood that not only the melting point of the initial silicon material layer 105 is lower than the melting point of the underlying silicon 104, but the melting point of the silicon film layer 114 is also lower than the melting point of the underlying silicon 104. Therefore, in the step of using laser to process the initial silicon material layer 105, the initial silicon material layer 105 and the silicon film layer 114 will both melt, and subsequently the initial silicon material layer 105 and the silicon film layer 114 in a molten state, that is, the layer to be crystallized 106, are cooled and recrystallized to form a silicon material layer.
[0068] In addition, in the step of using laser to process the initial silicon material layer 105, the laser heating temperature can be controlled. When the initial silicon material layer 105 and the silicon film layer 114 melt, the underlying silicon 104 also melts. In the subsequent cooling and recrystallization process of the molten initial silicon material layer 105 and the molten silicon film layer 114, the molten underlying silicon 104 is farthest from the heat source and crystallizes first. Therefore, the underlying silicon 104 that has been crystallized first is beneficial to providing better recrystallization conditions for the initial silicon material layer 105 and the silicon film layer 114 that are still in a molten state.
[0069] In some embodiments, the materials of the initial silicon material layer 105 and the silicon film layer 114 may both be polysilicon.
[0070] In some embodiments, in conjunction with reference Fig.11 and Fig.12 In the step of using laser to process the initial silicon material layer 105, the voids 115 in the initial silicon material layer 105 are eliminated. This is conducive to ensuring that there are no macroscopic void defects in the silicon material layer formed based on the molten initial silicon material layer 105, so as to improve the film uniformity and conductive performance of the silicon material layer.
[0071] In addition, since the laser can achieve the effect of local heating, the laser can generate relatively high temperatures in both the initial silicon material layer 105 and the silicon film layer 114. At this time, the temperature generated in other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 is relatively low, that is, the laser has a relatively small impact on the temperature values generated in other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114; and since the laser can achieve the effect of rapid heating, that is, the high temperature lasts for a relatively short time in the initial silicon material layer 105 and the silicon film layer 114, the time for the temperature impact on other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 is also relatively short. Therefore, even if the initial silicon material layer 105 and the silicon film layer 114 are in a high-temperature molten state by using the laser, the temperature impact generated by the laser on other structures adjacent to the initial silicon material layer 105 and the silicon film layer 114 can be ignored, and will not have an adverse effect on other properties of the semiconductor structure.
[0072] The working mode of the laser is described in detail below through two embodiments.
[0073] In some embodiments, the laser operation mode may include pulsed laser, and the steps of using the laser to process the initial silicon material layer 105 may include: Fig.11 , aligned with the blind hole 110 (reference Figure 5 ) is subjected to N pulse laser treatments to achieve local heating of the initial silicon material layer 105 located in the blind hole 110, where N is a positive integer, and as the number of times increases, the energy density of the pulse laser remains unchanged or increases. It can be understood that N pulse laser treatments are performed on the initial silicon material layer 105, which is conducive to heating the initial silicon material layer 105 to a molten state, reducing the duration of the high temperature generated by the laser, and further avoiding the adverse effects of the high temperature on the semiconductor structure.
[0074] It can be understood that, in the case of the blind hole 110 (reference Figure 5 ) in the step of subjecting the initial silicon material layer 105 to N pulse laser treatments, the silicon film layer 114 and / or the underlying silicon 104 may also be melted.
[0075] In some embodiments, as the number of times increases, the energy density of the pulsed laser is constant at first and then gradually increases. When the energy density of the pulsed laser is constant, the initial silicon material layer 105 is preheated, and when the energy density of the pulsed laser increases, the melting of the initial silicon material layer 105 is accelerated. It can be understood that the heating treatment of the initial silicon material layer 105 by preheating first and then high-temperature heating is beneficial to reduce the excessive change of the temperature value of the initial silicon material layer 105 itself at the beginning while allowing the initial silicon material layer 105 to quickly heat up and be in a molten state, thereby further avoiding the phenomenon of increased defect density in the initial silicon material layer 105 caused by excessive temperature changes.
[0076] In some embodiments, the energy density of the pulsed laser can be in the range of 0.3 mJ / cm 2 ~0.7mJ / cm 2 For example, the energy density of a pulse laser is 0.35mJ / cm 2 , 0.4mJ / cm 2 , 0.45mJ / cm 2 , 0.5mJ / cm 2 、0.55mJ / cm 2 、0.6mJ / cm 2 or 0.65mJ / cm 2 .
[0077] In some embodiments, the wavelength of the laser pulse may be 532 nm. It is understood that the wavelength of the laser pulse is a key factor affecting the laser radiation depth. In the direction Z, the radiation depth of the laser with a wavelength of 532 nm ranges from 200 nm to 300 nm. It is understood that in practical applications, the laser radiation depth may also be controlled by combining the energy density of the laser and the time interval between different lasers.
[0078] In some embodiments, the pulse width of the laser pulse may be 10 ns, and it is understood that the duration of a single laser pulse is 10 ns. In other embodiments, the pulse width of the laser pulse may also be less than 10 ns.
[0079] In some embodiments, N is 1 to 10, that is, the number of times the initial silicon material layer 105 is processed by using the pulse laser may be 1 to 10 times in total.
[0080] In one example, N is 4. When the initial silicon material layer 105 is subjected to pulse laser treatment for the first time, the energy density of the pulse laser is 0.35 mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the second time, the energy density of the pulsed laser is 0.35 mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the third time, the energy density of the pulsed laser is 0.4 mJ / cm 2 When the initial silicon material layer 105 is pulsed laser treated for the fourth time, the energy density of the pulsed laser is 0.45 mJ / cm 2 In addition, the interval between the first pulse laser treatment and the second pulse laser treatment is 100 ns, the interval between the second pulse laser treatment and the third pulse laser treatment is 50 ns, and the interval between the third pulse laser treatment and the fourth pulse laser treatment is 150 ns.
[0081] In another example, N is 4. When the initial silicon material layer 105 is subjected to pulse laser treatment for the first time, the surface temperature value of the initial silicon material layer 105 ranges from 690°C to 710°C; when the initial silicon material layer 105 is subjected to pulse laser treatment for the second time, the surface temperature value of the initial silicon material layer 105 ranges from 950°C to 970°C; when the initial silicon material layer 105 is subjected to pulse laser treatment for the third time, the surface temperature value of the initial silicon material layer 105 ranges from 990°C to 1010°C; when the initial silicon material layer 105 is subjected to pulse laser treatment for the fourth time, the surface temperature value of the initial silicon material layer 105 ranges from 1290°C to 1310°C. In addition, the interval between the first pulse laser treatment and the second pulse laser treatment is 40ns, the interval between the second pulse laser treatment and the third pulse laser treatment is 240ns, and the interval between the third pulse laser treatment and the fourth pulse laser treatment is 40ns.
[0082] In some embodiments, the total time duration for processing the initial silicon material layer with the laser pulses may be 1000 ns.
[0083] In some embodiments, in the step of treating the initial silicon material layer 105 with a laser pulse, the maximum temperature of the initial silicon material layer 105 is 1100° C. to 1400° C. This helps to ensure that when the initial silicon material layer 105 is in a molten state, the bottom silicon 104 will not melt, and subsequently serve as a seed layer when the molten initial silicon material layer 105 recrystallizes.
[0084] In some embodiments, in the step of processing the initial silicon material layer 105 with a laser pulse, the maximum depth of the melted initial silicon material layer 105 is 400nm to 500nm along the depth direction Z of the blind hole 110. This helps to avoid other devices deeper in the bottom of the semiconductor structure from being affected by temperature along the direction Z and away from the laser.
[0085] In other embodiments, the working mode of the laser may include continuous laser, and the step of using laser to process the initial silicon material layer 105 may include: using continuous laser to scan the substrate 100 and the initial silicon material layer 105, and the energy density of the continuous laser when scanning the substrate 100 is a first energy density, and the energy density of the continuous laser when scanning the initial silicon material layer 105 is a second energy density, and the first energy density is lower than the second energy density.
[0086] In the above embodiment, it can be understood that the laser irradiates the surface of the initial silicon material layer 105, and the surface of the initial silicon material layer 105 absorbs the laser energy, so that the temperature of the initial silicon material layer 105 rises to exceed its melting point, and then the initial silicon material layer 105 begins to be partially in a molten state, and the heat gradually diffuses along the direction Z and away from the laser, so that the liquid silicon / amorphous silicon interface moves downward, and finally the initial silicon material layer 105 is in a molten state as a whole. In addition, on the basis of the formation of the silicon film layer 114, in the above laser processing step, the silicon film layer 114 will also gradually melt until the entire layer is in a molten state.
[0087] S105: Combined with reference Figures 11 to 13 , the initial silicon material layer 105 after the laser treatment is cooled to make the initial silicon material layer 105 recrystallize to form a silicon material layer 107 .
[0088] In some embodiments, after the silicon film layer 114 is formed, in the step of recrystallizing the initial silicon material layer 105 , the silicon film layer 114 in a molten state and the initial silicon material layer 105 in a molten state are recrystallized together.
[0089] It is understandable that, combined with reference Fig.12 and Fig.13 After the layer to be crystallized 106 is formed, the laser treatment is stopped and the layer to be crystallized 106 is cooled. Figure 5 ) The bottom silicon 104 at the bottom is a seed layer, and the layer to be crystallized 106 is recrystallized with the bottom silicon 104 as the seed layer until the layer to be crystallized 106 is completely recrystallized to form a silicon material layer 107. It should be noted that, Fig.12 In the figure, the initial silicon material layer 105 in a molten state and the silicon film layer 114 in a molten state are uniformly drawn as a layer to be crystallized 106. Fig.13 In the figure, the layer to be crystallized 106 after all recrystallization is completed is drawn as a silicon material layer 107 .
[0090] In some embodiments, cooling the initial silicon material layer 105 after the laser treatment includes blowing an inert gas toward the initial silicon material layer 105 after the laser treatment. The inert gas may include at least one of nitrogen or argon.
[0091] In some embodiments, the pressure of the inert gas ranges from 0.2 MPa to 1 MPa.
[0092] In some other embodiments, the cooling treatment of the initial silicon material layer 105 after the laser treatment may be: allowing the initial silicon material layer 105 after the laser treatment to cool naturally.
[0093] In some embodiments, the silicon material layer 107 includes at least one of monocrystalline silicon or polycrystalline silicon, and the defect density of the silicon material layer 107 is lower than the defect density of the initial silicon material layer 105. In this way, when the capacitor contact layer, the bit line contact layer or other electrical contact layer is subsequently prepared using the silicon material layer 107 as a raw material, it is beneficial to improve the conductive performance of the film layer and ensure that it has a lower defect density.
[0094] It can be understood that since the melting point of the initial silicon material layer 105 is lower than the melting point of the underlying silicon 104, the initial silicon material layer 105 is in a molten state when heated, which can make the underlying silicon 104 in a non-molten state. Then, during the cooling and recrystallization process of the molten initial silicon material layer 105, the molten initial silicon material layer 105 can use the underlying silicon 104 as a seed layer and recrystallize along the crystal orientation of the crystals in the underlying silicon 104, so that the finally formed silicon material layer 107 includes at least one of single crystal silicon or polycrystalline silicon, which is beneficial to improve the density of the silicon material layer 107.
[0095] In some embodiments, after forming the silicon material layer 107, the method for manufacturing the semiconductor structure may further include: referring to Fig.13 , chemical mechanical polishing is performed on the silicon material layer 107; Fig.13 , the silicon material layer 107 is etched back, and the remaining silicon material layer 107 is used as an electrical contact layer, and the electrical contact layer is located at a blind hole 110 at a partial depth (reference Figure 5 )middle.
[0096] It should be noted that Fig.13 The silicon material layer 107 is shown after chemical mechanical polishing.
[0097] In summary, on the one hand, using laser to heat the initial silicon material layer 105 is conducive to avoiding the existence of voids or gaps in the silicon material layer 107 formed by the subsequent melting and recrystallization of the initial silicon material layer 105, thereby improving the compactness and conductivity of the silicon material layer 107; on the other hand, before forming the initial silicon material layer 105, a bottom silicon 104 is formed at the bottom of the blind hole 110 to provide the initial silicon material layer 105 with better recrystallization conditions, thereby facilitating the formation of a silicon material layer 107 with a lower defect density; on the other hand, since the laser can achieve the effect of local heating and the laser can achieve the effect of rapid heating, when the initial silicon material layer 105 is in a high-temperature molten state by using the laser, the temperature effect of the laser on other structures adjacent to the initial silicon material layer 105 can be ignored, and will not cause adverse effects on other properties of the semiconductor structure. Therefore, the manufacturing method of the semiconductor structure provided by an embodiment of the present disclosure is conducive to avoiding the process of forming the silicon material layer 107 from causing adverse effects on other parts of the semiconductor structure while improving the compactness and conductivity of the silicon material layer 107 formed.
[0098] Another embodiment of the present disclosure further provides a semiconductor structure, which is formed by the manufacturing method provided in one embodiment of the present disclosure. The semiconductor structure provided in another embodiment of the present disclosure will be described in detail below in conjunction with the accompanying drawings. It should be noted that the same or corresponding parts as the above embodiments are not repeated here.
[0099] Combined with reference Fig.14 The semiconductor structure includes: a substrate 100, the substrate 100 has at least one blind hole 110 (refer to Figure 5 ); the silicon material layer 107 is at least located at the bottom and part of the sidewall of the blind hole 110, and the defect density of the silicon material layer 107 is lower than the defect density of amorphous silicon.
[0100] In some embodiments, the silicon material layer 107 includes at least one of single crystal silicon or polycrystalline silicon. When the silicon material layer 107 is subsequently used as a capacitor contact layer, a bit line contact layer or other electrical contact layer, it is beneficial to improve the conductive properties of the film layer and ensure that it has a lower defect density, thereby helping to improve the yield of the semiconductor structure and device performance.
[0101] In some embodiments, in conjunction with reference Figure 5 and Fig.14 The base 100 may include: a substrate 101; a plurality of bit lines 102 arranged in parallel on the substrate 101 and a dielectric layer 103 located between adjacent bit lines 102, the dielectric layer 103 and the bit lines 102 together enclose a plurality of blind holes 110; along the extension direction Z of the blind holes 110, a silicon material layer 107 is located in the blind holes 110 at a partial depth.
[0102] It should be noted that Fig.14 This is only a specific application scenario of the finally formed silicon material layer 107 . In practical applications, the silicon material layer 107 formed by the manufacturing method provided by an embodiment of the present disclosure includes but is not limited to being used as a capacitor contact layer.
[0103] In summary, in the semiconductor structure formed by the manufacturing method provided in an embodiment of the present disclosure, the defect density of the silicon material layer 107 is lower than the defect density of amorphous silicon, which is beneficial to improving the yield rate and device performance of the semiconductor structure.
[0104] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present disclosure, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the embodiments of the present disclosure. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the embodiments of the present disclosure, so the protection scope of the embodiments of the present disclosure shall be based on the scope defined in the claims.
Claims
1. A method for manufacturing a semiconductor structure, characterized in that: include: providing a substrate having at least one blind hole therein; Using an epitaxial growth process to form a bottom layer of silicon at least at the bottom of the blind hole; forming an initial silicon material layer filling the remaining blind holes, wherein the melting point of the initial silicon material layer is lower than the melting point of the bottom silicon; Processing the initial silicon material layer with a laser to melt the initial silicon material layer; The initial silicon material layer after the laser treatment is cooled to allow the initial silicon material layer to recrystallize, thereby forming a silicon material layer.
2. The manufacturing method according to claim 1, characterized in that In the step of processing the initial silicon material layer with laser, voids in the initial silicon material layer are eliminated.
3. The manufacturing method according to claim 1, characterized in that: The silicon material layer includes at least one of single crystal silicon or polycrystalline silicon, and a defect density of the silicon material layer is lower than a defect density of the initial silicon material layer.
4. The manufacturing method according to claim 1, characterized in that: The working mode of the laser includes pulsed laser, and the processing of the initial silicon material layer by using the laser includes: The initial silicon material layer located in the blind hole is sequentially subjected to N pulse laser treatments to achieve local heating of the initial silicon material layer located in the blind hole, wherein N is a positive integer, and as the number of times increases, the energy density of the pulse laser remains unchanged or increases.
5. The manufacturing method according to claim 4, characterized in that: The energy density of the pulse laser is in the range of 0.3 mJ / cm 2 ~0.7mJ / cm 2 The wavelength of the laser pulse is 532 nm, and the pulse width of the laser pulse is 10 ns.
6. The manufacturing method according to claim 4, characterized in that: As the number of times increases, the energy density of the pulse laser remains unchanged at first and then gradually increases. When the energy density of the pulse laser remains unchanged, the initial silicon material layer is preheated, and when the energy density of the pulse laser increases, the melting of the initial silicon material layer is accelerated.
7. The manufacturing method according to any one of claims 1 to 6, characterized in that: In the step of processing the initial silicon material layer with laser pulses, the maximum value of the temperature of the initial silicon material layer is 1100° C. to 1400° C.
8. The manufacturing method according to any one of claims 1 to 6, characterized in that: In the step of processing the initial silicon material layer with laser pulses, the maximum depth of the melted initial silicon material layer along the depth direction of the blind hole is 400 nm to 500 nm.
9. The manufacturing method according to claim 1, characterized in that: Before forming the bottom silicon layer, the method further includes: cleaning the substrate.
10. The manufacturing method according to claim 1 or 9, characterized in that: In the step of forming a bottom layer of silicon at least at the bottom of the blind hole by using an epitaxial growth process, a silicon film layer is formed on the sidewall of the blind hole; The bottom silicon layer and the silicon film layer together enclose a contact hole, and the forming of an initial silicon material layer filling the blind hole comprises: forming an initial silicon material layer filling the contact hole; In the step of using laser to process the initial silicon material layer, the silicon film layer is also melted; In the step of recrystallizing the initial silicon material layer, the silicon film layer in a molten state and the initial silicon material layer in a molten state are recrystallized together.
11. The manufacturing method according to claim 1 or 9, characterized in that: Along the depth direction of the blind hole, the thickness of the bottom silicon is in the range of 1 nm to 5 nm.
12. The manufacturing method according to claim 1, characterized in that: The cooling process includes blowing an inert gas toward the initial silicon material layer after the laser treatment, and the pressure of the inert gas has a numerical range of 0.2 MPa to 1 MPa.
13. The manufacturing method according to claim 1, characterized in that: The step of providing the substrate comprises: providing a substrate; A plurality of bit lines arranged in parallel and a dielectric layer located between adjacent bit lines are formed on the substrate, wherein the dielectric layer and the bit lines together enclose a plurality of blind holes, and the blind holes are capacitor contact holes; Alternatively, a plurality of grooves for forming bit lines are formed in the substrate, the grooves have the blind holes therein, and the blind holes are used to form bit line contact layers.
14. A semiconductor structure, characterized in that: include: a substrate having at least one blind hole therein; The silicon material layer is at least located at the bottom and part of the sidewall of the blind hole, and the defect density of the silicon material layer is lower than the defect density of amorphous silicon.
15. The semiconductor structure according to claim 14, wherein: The substrate comprises: substrate; A plurality of bit lines arranged in parallel on the substrate and a dielectric layer located between adjacent bit lines, wherein the dielectric layer and the bit lines together enclose a plurality of blind holes; Along the extension direction of the blind hole, the silicon material layer is located in a partial depth of the blind hole.