Flash memory device and preparation method thereof
By etching the logic area first and then the storage area in semiconductor manufacturing, and using ISSG and HARP processes to process the inner walls of the trenches, the problems of poor corner rounding in the peripheral logic area and over-oxidation of the floating gate layer are solved, improving the performance of flash memory devices. electrical performance and reliability.
Patent Information
- Application Number
- CN202410825323.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-25
- Publication Date
- 2024-10-11
AI Technical Summary
In semiconductor manufacturing, the poor corner rounding effect in the active area of the peripheral logic area of the 55nm ETOX Nor Flash structure causes MOS tube leakage, and the high-density plasma process in the traditional FG-first process affects device reliability.
Using the etching sequence of first the logic area and then the storage area, a sacrificial oxide layer is formed on the inner wall of the trench through the ISSG process and wet removed, and then a liner oxide layer is formed, combined with the HARP process to form an isolation material layer to avoid high-density plasma damage to the reliability Negative effects of sex.
It improves the leakage problem of MOS tubes, ensures the uniform oxidation thickness and film quality of the floating gate layer, and improves the reliability and product yield of the device.
Smart Images

Figure CN118765113A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor manufacturing technology, and in particular to a flash memory device and a method for preparing the same. Background Art
[0002] The 55nm ETOX (Erase Through Oxide) Nor Flash (non-volatile memory) structure is shrinking to smaller nodes (<=45nm). Considering the problems of filling two layers of Poly (floating gate and control gate), the FG-first technology route needs to be adopted.
[0003] Among them, the traditional process flow of the FG-first technology route is roughly as follows: first, a tunneling oxide layer, a floating gate polysilicon layer (FG) and a hard mask layer are deposited on the substrate, and then the active area of the storage area is etched to form a storage area isolation trench, and then the active area of the peripheral logic area is etched to form a logic area isolation trench, and then a pad oxide layer is deposited in the storage area isolation trench and the logic area isolation trench through an oxidation process, and at the same time, the top corners (corners) of different film layers on the inner walls of the storage area isolation trench and the logic area isolation trench are made into rounded corners.
[0004] Since the peripheral logic area belongs to the typical logic circuit area, the requirements for rounding the corners of the active area of the peripheral logic area are high. Poor rounding of the corners of the active area of the peripheral logic area will cause leakage of the MOS tube, and the CP (Chip Probing) test will show BIN5 (ISB) fail. However, if the thickness of the pad oxide layer is simply increased, the floating gate polysilicon layer in the storage area will be excessively oxidized, thereby affecting the storage device in the storage area. In addition, in order to avoid the oxidation and deformation of the floating gate polysilicon layer caused by the steam annealing process in the HARP (High Aspect Ratio Process) process, the traditional FG-first process usually uses the HDP (High Density Plasma) process to fill the isolation layer of the trench, but high-density plasma can easily cause the reliability of the device to decrease. Summary of the invention
[0005] The present application provides a flash memory device and a method for preparing the same, which can solve at least one of the following problems: MOS tube leakage caused by poor rounding effect of the corners of the active area in the peripheral logic area of the flash memory device, overoxidation or oxidation deformation of the floating gate polysilicon layer in the storage area of the flash memory device, and poor reliability of the flash memory device.
[0006] On the one hand, an embodiment of the present application provides a method for preparing a flash memory device, comprising:
[0007] A substrate is provided, wherein the substrate comprises a storage area and a logic area, and a tunneling oxide layer, a floating gate layer and a hard mask layer are formed on the substrates of the storage area and the logic area;
[0008] Etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the logic region to form a plurality of first trenches;
[0009] An ISSG process is used to form a sacrificial oxide layer, wherein the top corners of the substrate and the top corners of the floating gate layer are exposed on the sidewall surface of the first trench, and the sacrificial oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewall of the first trench;
[0010] Removing the sacrificial oxide layer using a wet cleaning process;
[0011] An ISSG process is used to form a first liner oxide layer, wherein the first liner oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench, wherein the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench are both arc-shaped;
[0012] forming a first isolation material layer, wherein the first isolation material layer covers the first liner oxide layer and fills the first trench;
[0013] Etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the storage area to form a plurality of second trenches;
[0014] forming a second pad oxide layer, wherein the second pad oxide layer covers the hard mask layer, the sidewalls and bottom wall of the second trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench;
[0015] A second isolation material layer is formed, wherein the second isolation material layer covers the second liner oxide layer and fills the second trench.
[0016] Optionally, in the method for preparing the flash memory device, in the process of forming the sacrificial oxide layer by adopting the ISSG process, the process temperature is 800° C. to 1300° C.; and the gases involved in the reaction include: H2 and O2.
[0017] Optionally, in the method for preparing the flash memory device, in the process of forming the first liner oxide layer by adopting the ISSG process, the process temperature is 800° C. to 1300° C.; and the gases involved in the reaction include: H2 and O2.
[0018] Optionally, in the method for preparing the flash memory device, the thickness of the first pad oxide layer is greater than the thickness of the second pad oxide layer.
[0019] Optionally, in the preparation method of the flash memory device, the second pad oxide layer is formed by an ISSG process so that the side wall surface of the second trench exposes the top edge corners of the substrate and the top edge corners of the floating gate layer, and the top edge corners of the substrate and the top edge corners of the floating gate layer on the side wall of the second trench are rounded.
[0020] Optionally, in the method for preparing the flash memory device, the first isolation material layer is formed by a HARP process.
[0021] Optionally, in the method for preparing the flash memory device, after forming the first isolation material layer and before forming the second trench, the method for preparing the flash memory device further includes:
[0022] The first liner oxide layer on the surface of the hard mask layer and the first isolation material layer beyond the surface of the hard mask layer are polished and removed by using a CMP process.
[0023] Optionally, in the method for preparing the flash memory device, after forming the second isolation material layer, the method for preparing the flash memory device further includes:
[0024] The second liner oxide layer on the surface of the hard mask layer and the second isolation material layer beyond the surface of the hard mask layer are polished and removed by using a CMP process.
[0025] Optionally, in the method for preparing the flash memory device, the second isolation material layer is formed by a HDP process.
[0026] On the other hand, an embodiment of the present application further provides a flash memory device, including:
[0027] A substrate, the substrate comprising a storage area and a logic area, and a tunneling oxide layer, a floating gate layer and a hard mask layer are formed on the substrates of the storage area and the logic area;
[0028] A plurality of first trenches, wherein the first trenches are located in the hard mask layer, the floating gate layer, the tunnel oxide layer and a portion of the thickness of the substrate in the logic region, and the sidewall surfaces of the first trenches expose the top corners of the substrate and the top corners of the floating gate layer;
[0029] a first liner oxide layer, wherein the first liner oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench, wherein the first liner oxide layer is formed by an ISSG process, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench are both arc-shaped;
[0030] A first isolation material layer, the first isolation material layer covers the first liner oxide layer and fills the first trench;
[0031] a plurality of second trenches, wherein the second trenches are located in the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the storage region;
[0032] a second pad oxide layer, wherein the second pad oxide layer covers the hard mask layer, the sidewalls and bottom wall of the second trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench; and
[0033] A second isolation material layer covers the second liner oxide layer and fills the second trench.
[0034] The technical solution of this application has at least the following advantages:
[0035] The present application first etches the logic area and then etches the storage area, wherein in the active area process of the logic area, a sacrificial oxide layer is first formed on the inner wall of the first trench by the ISSG process to strengthen the rounding effect of the top corners of the substrate and the top corners of the floating gate layer on the side wall of the first trench, then the sacrificial oxide layer is removed by a wet method, and the first liner oxide layer is formed on the inner wall of the first trench by the ISSG process again, which can not only further strengthen the rounding effect of the top corners of the substrate and the top corners of the floating gate layer on the side wall of the first trench, making the top corners of the substrate and the top corners of the floating gate layer on the side wall of the first trench more rounded, but also obtain a first liner oxide layer with higher thickness uniformity and better film quality, which can improve the leakage of the MOS tube; further, because the deposition of the liner oxide layer of the logic area is first performed and the deposition of the liner oxide layer of the storage area is performed later, the side surface of the floating gate layer in the storage area is avoided from being over-oxidized, the coupling ratio of the control gate and the floating gate is guaranteed, and the storage area device is guaranteed not to be affected.
[0036] Furthermore, the present application adopts the HARP process to form the first isolation material layer, which can avoid the impact of high-density plasma (HDP plasma) on the reliability of peripheral area devices, ensure the reliability of the devices, and improve the product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] In order to more clearly illustrate the specific implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0038] Figure 1 is a flow chart of a method for preparing a flash memory device according to an embodiment of the present invention;
[0039] Figure 2-Figure 10 is a schematic diagram of a semiconductor structure in each process step of preparing a flash memory device according to an embodiment of the present invention;
[0040] The reference numerals are described as follows:
[0041] 10 - substrate, 20 - tunneling oxide layer, 30 - floating gate layer, 40 - hard mask layer, 51 - first trench, 52 - second trench, 60 - sacrificial oxide layer, 71 - first pad oxide layer, 72 - second pad oxide layer, 81 - first isolation material layer, 82 - second isolation material layer. DETAILED DESCRIPTION
[0042] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in this application. Obviously, the described embodiments are part of the embodiments of this application, not all of them. Based on the embodiments in this application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0043] In the description of the present application, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present application. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0044] In the description of this application, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, it can also be the internal connection of two components, it can be a wireless connection, or it can be a wired connection. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0045] In addition, the technical features involved in the different embodiments of the present application described below can be combined with each other as long as they do not conflict with each other.
[0046] The present application provides a method for preparing a flash memory device, referring to Figure 1 , Figure 1 1 is a flow chart of a method for preparing a flash memory device according to an embodiment of the present invention, wherein the method for preparing a flash memory device comprises:
[0047] Step S1: providing a substrate, wherein the substrate comprises a storage area and a logic area, and a tunneling oxide layer, a floating gate layer and a hard mask layer are formed on the substrates of the storage area and the logic area;
[0048] Step S2: etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a portion of the thickness of the substrate in the logic area to form a plurality of first trenches;
[0049] Step S3: forming a sacrificial oxide layer by using an ISSG process, wherein the top corners of the substrate and the top corners of the floating gate layer are exposed on the sidewall surface of the first trench, and the sacrificial oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewall of the first trench;
[0050] Step S4: removing the sacrificial oxide layer by a wet cleaning process;
[0051] Step S5: forming a first liner oxide layer by using an ISSG process, wherein the first liner oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench, wherein the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench are both arc-shaped;
[0052] Step S6: forming a first isolation material layer, wherein the first isolation material layer covers the first liner oxide layer and fills the first trench;
[0053] Step S7: etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a portion of the thickness of the substrate in the storage area to form a plurality of second trenches;
[0054] Step S8: forming a second pad oxide layer, wherein the second pad oxide layer covers the hard mask layer, the sidewalls and bottom wall of the second trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench;
[0055] Step S9: forming a second isolation material layer, wherein the second isolation material layer covers the second liner oxide layer and fills the second trench.
[0056] Specifically, refer to Figure 2-Figure 10 , Figure 2-Figure 10 It is a schematic diagram of the semiconductor structure in each process step of preparing a flash memory device according to an embodiment of the present invention.
[0057] First, perform step S1: refer to Figure 2 , Figure 2 It is a schematic diagram of the semiconductor structure after the hard mask layer is formed in an embodiment of the present application, providing a substrate 10, the substrate 10 comprising a storage area and a logic area, and a tunneling oxide layer 20, a floating gate layer 30 and a hard mask layer 40 are formed on the substrate 10 of the storage area and the logic area.
[0058] Then, execute step S2: refer to Figure 3 , Figure 3 It is a schematic diagram of the semiconductor structure after the first trench is formed in an embodiment of the present application, wherein the hard mask layer 40 , the floating gate layer 30 , the tunneling oxide layer 20 and a partial thickness of the substrate 10 in the logic area are etched to form a plurality of first trenches 51 .
[0059] Specifically, an anti-reflective coating and a photoresist layer can be first formed on the surface of the hard mask layer 40, and then a first groove pattern can be formed on the photoresist layer through a photolithography process. Subsequently, the photoresist layer formed with the first groove pattern is used as a mask to etch the hard mask layer 40, the floating gate layer 30, the tunneling oxide layer 20 and a partial thickness of the substrate 10 in the logic area to form a plurality of first grooves 51, and finally the photoresist layer and the anti-reflective coating are removed.
[0060] Next, execute step S3: refer to Figure 4 , Figure 41 is a schematic diagram of a semiconductor structure after a sacrificial oxide layer is formed in an embodiment of the present application. The sacrificial oxide layer 60 is formed by an ISSG (In-Situ Steam Generation) process. At this time, the side wall surface of the first trench 51 exposes the top corners of the substrate 10, the corners of the tunneling oxide layer 20, and the top corners of the floating gate layer 30. Moreover, through the ISSG process, the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer exposed on the side wall surface of the first trench are transformed from sharp corners to rounded corners. The sacrificial oxide layer 60 covers the hard mask layer 40, the bottom wall of the first trench 51, and the entire side wall of the first trench 51, wherein the sacrificial oxide layer 60 covers the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer on the side wall of the first trench 51.
[0061] Preferably, in the process of forming the sacrificial oxide layer 60 by adopting the ISSG process, the process temperature is 800° C. to 1300° C.; the gases involved in the reaction include: H 2 and O 2 .
[0062] Preferably, the thickness of the sacrificial oxide layer 60 is
[0063] Among them, due to the different oxidation rates on the surfaces of different film layers, the ISSG process utilizes the strong oxidizing property of atomic oxygen to make the top corners of the substrate and the top corners of the floating gate layer on the side wall surface of the second trench protrude, and can effectively repair the contours of the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer exposed on the side wall surface of the first trench. At this time, the contours of the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer exposed on the side wall surface of the first trench are all transformed from sharp corners to rounded corners. At the same time, the ISSG process also reduces defects in the substrate and the tunneling oxide layer on the side wall surface of the first trench, thereby improving the quality and electrical properties of the substrate and the tunneling oxide layer on the side wall surface of the first trench.
[0064] Further, step S4 is performed: refer to Figure 5 , Figure 5 Schematic diagram of the semiconductor structure after the sacrificial oxide layer is removed by wet cleaning according to an embodiment of the present application. The sacrificial oxide layer 60 is removed by wet cleaning process.
[0065] In the present application, a wet cleaning process is used to remove the sacrificial oxide layer 60, which can further adjust the contours of the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer exposed on the side wall surface of the first groove, so that the arcs of the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer on the side wall surface of the first groove are smoother.
[0066] Next, execute step S5: refer to Figure 6 , Figure 6 It is a schematic diagram of the semiconductor structure after the first pad oxide layer is formed in an embodiment of the present application. The first pad oxide layer 71 is formed by the ISSG process. The first pad oxide layer 71 covers the hard mask layer 40, the bottom wall and side wall of the first trench 51, and the top corners of the substrate, the corners of the tunneling oxide layer, and the top corners of the floating gate layer on the side walls of the first trench 51, wherein the top corners between the tunneling oxide layer and the substrate on the side walls of the first trench and the top corners of the floating gate layer are both arc-shaped.
[0067] Preferably, in the process of forming the first liner oxide layer 71 by adopting the ISSG process, the process temperature is 800° C. to 1300° C.; the gases involved in the reaction include: H 2 and O 2 .
[0068] Preferably, the thickness of the first liner oxide layer 71 is
[0069] In the present application, the ISSG process is used to form the first pad oxide layer, and the strong oxidizing property of atomic oxygen is continued to be used to further repair the side wall surface of the first trench to expose the top corners of the substrate, the corners of the tunneling oxide layer and the top corners of the floating gate layer, so that the top corners of the substrate, the corners of the tunneling oxide layer and the top corners of the floating gate layer on the side walls of the second trench are all transformed into rounded corners, which is beneficial to the subsequent filling of the first isolation material layer and avoids the occurrence of void defects when filling the first isolation material layer.
[0070] Further, step S6 is performed: refer to Figure 7 , Figure 7 It is a schematic diagram of the semiconductor structure after forming the first isolation material layer according to an embodiment of the present application, wherein the first isolation material layer 81 is formed, and the first isolation material layer 81 covers the first liner oxide layer 71 and fills the first trench 51 .
[0071] In this embodiment, the first isolation material layer 81 is made of silicon dioxide.
[0072] Preferably, the first isolation material layer 81 is formed by using a HARP process. The present application uses a HARP process to form the first isolation material layer, which can avoid the impact of high-density plasma (HDP plasma) on the reliability of peripheral area devices, ensure the reliability of the device, and improve the product yield.
[0073] Furthermore, after forming the first isolation material layer 81, the preparation method of the flash memory device may also include: using a CMP process to grind and remove the first pad oxide layer 71 on the surface of the hard mask layer 40 and the first isolation material layer 81 extending beyond the surface of the hard mask layer 40, leaving only the first isolation material layer 81 in the first groove 51.
[0074] Next, execute step S7: refer to Figure 8 , Figure 8 It is a schematic diagram of the semiconductor structure after the second trench is formed in an embodiment of the present application, wherein the hard mask layer 40 , the floating gate layer 30 , the tunneling oxide layer 20 and a partial thickness of the substrate 10 in the storage area are etched to form a plurality of second trenches 52 .
[0075] Specifically, an anti-reflective coating and a photoresist layer may be first formed on the surface of the hard mask layer 40, and then a second groove pattern may be formed on the photoresist layer through a photolithography process. At this time, the logic area is completely covered by the photoresist layer. Next, the photoresist layer having the second groove pattern is used as a mask to etch the hard mask layer 40, the floating gate layer 30, the tunneling oxide layer 20 and a partial thickness of the substrate 10 in the logic area to form a plurality of second grooves 52, and finally the photoresist layer and the anti-reflective coating are removed.
[0076] Further, step S8 is performed: refer to Fig. 9 , Fig. 9 It is a schematic diagram of the semiconductor structure after the second pad oxide layer is formed in an embodiment of the present application, wherein the second pad oxide layer 72 is formed, and the second pad oxide layer 72 covers the hard mask layer 40, the side walls and bottom walls of the second trench 52, and the top corners of the substrate and the top corners of the floating gate layer on the side walls of the second trench 52.
[0077] Preferably, the thickness of the first liner oxide layer 71 is greater than the thickness of the second liner oxide layer 72 .
[0078] Preferably, the second liner oxide layer 72 is formed by the ISSG process. Through the ISSG process, the top corners of the substrate exposed on the sidewall surface of the second groove, the corners of the tunneling oxide layer and the top corners of the floating gate layer are transformed from sharp corners to rounded corners, which is beneficial to the subsequent filling of the second isolation material layer and avoids the occurrence of void defects when filling the second isolation material layer.
[0079] Finally, execute step S9: reference Fig.10 , Fig.10 It is a schematic diagram of the semiconductor structure after forming the second isolation material layer according to an embodiment of the present application. The second isolation material layer 82 is formed. The second isolation material layer 82 covers the second liner oxide layer 72 and fills the second trench 52 .
[0080] In this embodiment, the second isolation material layer 82 is made of silicon dioxide.
[0081] Preferably, the second isolation material layer 82 is formed by using a HDP process.
[0082] In the present application, etching, filling and other processes of the first trench of the logic area are first performed, and then etching, filling and other processes of the second trench of the storage area are performed. In the active area process of the logic area, a sacrificial oxide layer is first formed on the inner wall of the first trench by the ISSG process to strengthen the rounded corner effect of the top edge corner of the substrate on the side wall of the first trench, and then the sacrificial oxide layer is removed by a wet method, and the first liner oxide layer is formed on the inner wall of the first trench by the ISSG process again. This can not only further strengthen the rounded corner effect of the top edge corner of the substrate on the side wall of the first trench, making the top edge corner of the substrate on the side wall of the first trench more rounded, but also obtain a first liner oxide layer with higher thickness uniformity and better film quality, thereby improving the leakage of the MOS tube and improving the electrical performance of the device; further, because the deposition of the liner oxide layer of the logic area is performed first and the deposition of the liner oxide layer of the storage area is performed later, the side surface of the floating gate layer in the storage area is avoided from being over-oxidized, the coupling ratio of the control gate and the floating gate is guaranteed, and the storage area device is guaranteed not to be affected.
[0083] Furthermore, after forming the second isolation material layer 82 , the method for preparing the flash memory device may further include: using a CMP process to grind and remove the second liner oxide layer 72 on the surface of the hard mask layer 40 and the second isolation material layer 82 beyond the surface of the hard mask layer 40 .
[0084] In this embodiment, the subsequent process may further include conventional process steps of existing ETOX Nor Flash devices, such as removing the hard mask layer 40 , depositing an ONO film layer, and depositing a control gate layer.
[0085] Based on the same inventive concept, the present application also provides a flash memory device, referring to Fig.10 , Fig.10 : is a schematic diagram of the structure of a flash memory device according to an embodiment of the present application, the flash memory device comprises:
[0086] A substrate 10, wherein the substrate comprises a storage area and a logic area, and a tunneling oxide layer 20, a floating gate layer 30 and a hard mask layer 40 are formed on the substrates of the storage area and the logic area;
[0087] A plurality of first trenches 51, wherein the first trenches 51 are located in the hard mask layer 40, the floating gate layer 30, the tunneling oxide layer 20 and a portion of the thickness of the substrate 10 in the logic region, and the sidewall surfaces of the first trenches 51 expose the top corners of the substrate 10, the corners of the tunneling oxide layer 20 and the top corners of the floating gate layer 30;
[0088] A first liner oxide layer 71, wherein the first liner oxide layer 71 covers the hard mask layer 40, the bottom wall of the first trench 51, and the top corners of the substrate 10, the corners of the tunneling oxide layer 20, and the top corners of the floating gate layer 30 on the sidewalls of the first trench 51, wherein the first liner oxide layer 71 is formed by an ISSG process, and the top corners of the substrate 10, the corners of the tunneling oxide layer 20, and the top corners of the floating gate layer 30 on the sidewalls of the first trench are all arc-shaped;
[0089] A first isolation material layer 81, wherein the first isolation material layer 81 covers the first liner oxide layer 71 and fills the first trench 51;
[0090] A plurality of second trenches 52, wherein the second trenches 52 are located in the hard mask layer 40, the floating gate layer 30, the tunnel oxide layer 20 and a partial thickness of the substrate 10 in the storage region;
[0091] a second liner oxide layer 72, wherein the second liner oxide layer 72 covers the hard mask layer 40, the sidewalls and bottom wall of the second trench 52, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench; and
[0092] A second isolation material layer 82 , where the second isolation material layer 82 covers the second liner oxide layer 72 and fills the second trench 52 .
[0093] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection created by this application.
Claims
1. A method for preparing a flash memory device, It is characterized in that include: A substrate is provided, wherein the substrate comprises a storage area and a logic area, and a tunneling oxide layer, a floating gate layer and a hard mask layer are formed on the substrates of the storage area and the logic area; Etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the logic region to form a plurality of first trenches; An ISSG process is used to form a sacrificial oxide layer, wherein the top corners of the substrate and the top corners of the floating gate layer are exposed on the sidewall surface of the first trench, and the sacrificial oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewall of the first trench; Removing the sacrificial oxide layer using a wet cleaning process; An ISSG process is used to form a first liner oxide layer, wherein the first liner oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench, wherein the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench are both arc-shaped; forming a first isolation material layer, wherein the first isolation material layer covers the first liner oxide layer and fills the first trench; Etching the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the storage area to form a plurality of second trenches; forming a second pad oxide layer, wherein the second pad oxide layer covers the hard mask layer, the sidewalls and bottom wall of the second trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench; A second isolation material layer is formed, wherein the second isolation material layer covers the second liner oxide layer and fills the second trench.
2. The method for preparing a flash memory device according to claim 1, It is characterized in that In the process of forming the sacrificial oxide layer by the ISSG process, the process temperature is 800° C. to 1300° C.; the gases involved in the reaction include: H 2 and O 2 .
3. The method for preparing a flash memory device according to claim 1, It is characterized in that In the process of forming the first liner oxide layer by adopting the ISSG process, the process temperature is 800° C. to 1300° C.; the gases involved in the reaction include: H 2 and O 2 .
4. The method for preparing a flash memory device according to claim 1, It is characterized in that The thickness of the first pad oxide layer is greater than the thickness of the second pad oxide layer.
5. The method for preparing a flash memory device according to claim 1, It is characterized in that The second liner oxide layer is formed by ISSG process so that the sidewall surface of the second trench exposes the top corners of the substrate and the top corners of the floating gate layer, and the top corners of the substrate and the top corners of the floating gate layer on the sidewall of the second trench are rounded.
6. The method for preparing a flash memory device according to claim 1, It is characterized in that The first isolation material layer is formed by adopting a HARP process.
7. The method for preparing a flash memory device according to claim 1, It is characterized in that After forming the first isolation material layer and before forming the second trench, the method for preparing the flash memory device further includes: The first liner oxide layer on the surface of the hard mask layer and the first isolation material layer beyond the surface of the hard mask layer are polished and removed by using a CMP process.
8. The method for preparing a flash memory device according to claim 1, It is characterized in that After forming the second isolation material layer, the method for preparing the flash memory device further includes: The second liner oxide layer on the surface of the hard mask layer and the second isolation material layer beyond the surface of the hard mask layer are polished and removed by using a CMP process.
9. The method for preparing a flash memory device according to claim 1, It is characterized in that The second isolation material layer is formed by adopting a HDP process.
10. A flash memory device, It is characterized in that include: A substrate, the substrate comprising a storage area and a logic area, and a tunneling oxide layer, a floating gate layer and a hard mask layer are formed on the substrates of the storage area and the logic area; A plurality of first trenches, wherein the first trenches are located in the hard mask layer, the floating gate layer, the tunnel oxide layer and a portion of the thickness of the substrate in the logic region, and the sidewall surfaces of the first trenches expose the top corners of the substrate and the top corners of the floating gate layer; a first liner oxide layer, wherein the first liner oxide layer covers the hard mask layer, the bottom wall of the first trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench, wherein the first liner oxide layer is formed by an ISSG process, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the first trench are both arc-shaped; A first isolation material layer, the first isolation material layer covers the first liner oxide layer and fills the first trench; a plurality of second trenches, wherein the second trenches are located in the hard mask layer, the floating gate layer, the tunnel oxide layer and a partial thickness of the substrate in the storage region; a second pad oxide layer, wherein the second pad oxide layer covers the hard mask layer, the sidewalls and bottom wall of the second trench, and the top corners of the substrate and the top corners of the floating gate layer on the sidewalls of the second trench; and A second isolation material layer covers the second liner oxide layer and fills the second trench.
Citation Information