Preparation method of high-temperature superconducting quantum interference device capable of accurately positioning bicrystal junction and crystal boundary
By forming a micron-level positioning mark structure on the high-temperature superconducting material layer and using a transmission microscope for alignment, the difficulty in aligning the Josephson microbridge junction and grain boundaries in high-temperature superconducting quantum interference devices is solved, achieving higher alignment. accuracy and yield.
Patent Information
- Application Number
- CN202410786818.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-11
AI Technical Summary
In the process of preparing high-temperature superconducting quantum interference devices, it is difficult to accurately locate the grain boundaries between the Josephson microbridge junction and the bicrystal substrate, especially due to the insufficient light source power of the transmission microscope and the low microscope magnification, resulting in high-quality grain boundaries. It is difficult to align accurately, affecting the noise characteristics and yield of the device.
A micron-level linear lattice positioning mark structure is formed on the high-temperature superconducting material layer. A transmission microscope is used to determine the relative position between the grain boundary and the positioning mark. The photoresist layer and exposure technology are used to form the positioning mark structure on the dual crystal substrate. Josephson microbridge junction, ensuring its alignment with grain boundaries.
The alignment accuracy, stability and repeatability of the small-sized Josephson junction and the grain boundary of the dual-crystal substrate are improved, and the production efficiency and yield of high-temperature superconducting quantum interference devices are significantly improved.
Smart Images

Figure CN118765156A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of superconducting electronics, and more specifically, to a method for preparing a high-temperature superconducting quantum interference device for accurately positioning a twin crystal junction and a grain boundary. Background Art
[0002] Superconducting quantum interference device (SQUID) is one of the most sensitive flux-to-voltage converters currently available. Due to its excellent performance, SQUID devices are mainly used in precision measurement and can measure weak physical quantities such as current, voltage, magnetic field, magnetic field gradient, and magnetic susceptibility. Currently, SQUID has been maturely applied in biomedicine, non-destructive testing, geophysical exploration, etc., and has extremely broad development prospects.
[0003] like Figure 1 As shown in the figure, inserting two Josephson junctions in a closed superconducting loop constitutes a DC SQUID. According to the superconducting material, SQUID is divided into low-temperature and high-temperature devices. Low-temperature devices usually use Nb / Al-AlOx / Nb Josephson junction devices, which are characterized by mature and stable technology and high sensitivity, but they require a low-temperature liquid helium environment when working, and the cost of use is relatively high. At the same time, my country's helium resources are basically dependent on imports. Except for the economically developed regions of Beijing, Shanghai and Guangzhou, there is rarely liquid helium, which greatly restricts the promotion of low-temperature SQUID technology. The superconducting materials used to prepare high-temperature superconducting SQUIDs, such as yttrium barium copper oxide (abbreviated as YBCO), thallium barium calcium copper oxide (TBCCO), bismuth strontium calcium copper oxide (BSCCO), etc., can avoid such problems. Because it works in the liquid nitrogen temperature range, the cost of use is low, the refrigeration facilities are small, and the measurement environment restrictions are small, which is convenient for field use.
[0004] At present, the preparation of high-temperature superconducting Josephson junctions mainly includes twin crystal junctions, step junctions and the use of focused helium ion beams to prepare Josephson junctions. Figure 2 As shown in the figure, the weak connection formed by grain boundaries with different orientations is called a twin crystal junction. After the crystal substrate used to grow the high-temperature superconducting film is oriented, two substrates with different orientations are aligned and sintered together at a certain angle (θ) to form a twin crystal substrate. A high-temperature superconducting film is epitaxially grown on the twin crystal substrate (the film orientation is consistent with the substrate orientation). Since the film orientations on the two substrates are inconsistent, a weak connection is formed at the grain boundary. The microbridge superconducting structure is crossed over the grain boundary to form a twin crystal junction. The advantages of using a twin crystal junction to prepare SQUID are a short process flow, high yield, and better noise characteristics. The disadvantage is that high-quality twin crystal substrates are expensive.
[0005] In the process of preparing the twin crystal junction, a Josephson junction with a length of less than 10 μm needs to accurately cross the grain boundary (GB) of the twin crystal substrate. Since the twin crystal substrate is a surface polished process after two crystal orientation substrates are sintered together, the grain boundary cannot be observed with a reflective microscope and can only be seen with a transmission microscope. However, conventional UV exposure machines use a reflective microscope for pre-exposure alignment. Therefore, when the SQUID pattern is transferred to a high-temperature superconducting film by exposure, the microbridge structure with a length of less than 10 μm cannot accurately cross the grain boundary of the twin crystal substrate. This is the biggest difficulty in preparing the twin crystal junction.
[0006] The current solution to this problem is to modify the photolithography machine. Replace the sample carrier with a transparent material, such as glass; replace the light source with a low-power infrared LED lamp and place it under the carrier to form a transmission optical alignment system. This system can complete most of the alignment functions of the twin crystals. However, since the power of the transmitted LED light source cannot be too high and the microscope magnification on the photolithography machine is low, this method is not always effective. In particular, after growing a black high-temperature superconducting film, it is also difficult to observe the grain boundaries with a transmission microscope, and the higher the quality of the grain boundaries, the harder it is to see the grain boundaries.
[0007] The information disclosed in the background technology section of the present invention is only intended to deepen the understanding of the general background technology of the present invention, and should not be regarded as acknowledging or suggesting in any form that the information constitutes the prior art already known to those skilled in the art. Summary of the invention
[0008] The purpose of the present invention is to provide a method for preparing a high-temperature superconducting quantum interference device that accurately positions a twin crystal junction and a grain boundary, so as to achieve precise alignment between a Josephson microbridge junction and a grain boundary of a twin crystal substrate during the preparation of a high-temperature superconducting quantum interference device.
[0009] To achieve the above objectives, in a first aspect, the present invention proposes a method for preparing a high-temperature superconducting quantum interference device for accurately positioning a twin crystal junction and a grain boundary, comprising:
[0010] Providing a double crystal substrate, on which a high temperature superconducting material layer is deposited, wherein the bonding interface between two substrates in the double crystal substrate is a grain boundary;
[0011] Forming a micrometer-scale linear dot matrix positioning mark structure on the high-temperature superconducting material layer near the grain boundary, wherein the straight line where the positioning mark structure is located is perpendicular to the extension direction of the grain boundary;
[0012] Determining the relative position between the grain boundary and the positioning mark by a transmission microscope;
[0013] forming a first photoresist layer covering the high temperature superconducting material layer and the positioning mark structure;
[0014] Using a layout with a superconducting quantum interference device structure, using the positioning mark structure to determine the position of the grain boundary, so that the center of the Josephson microbridge junction pattern in the layout is aligned with the grain boundary;
[0015] patterning the first photoresist layer by exposure and development;
[0016] The high-temperature superconducting material layer is etched using the patterned first photoresist layer as a mask to form a Josephson microbridge junction across the grain boundary on the bicrystalline substrate to form a high-temperature superconducting quantum interference device.
[0017] Optionally, the positioning mark structure includes a plurality of micrometer-level dot marks and a plurality of different digital marks;
[0018] The plurality of point-shaped marks are distributed at equal intervals along a direction perpendicular to the extension direction of the grain boundary, and the straight line segment where the plurality of point-shaped marks are located intersects the grain boundary perpendicularly;
[0019] The plurality of digital identifiers are periodically distributed on one side of the plurality of dot-shaped identifiers along a direction perpendicular to the extension direction of the grain boundaries, and the values of the plurality of digital identifiers are increased in sequence.
[0020] Optionally, determining the relative position between the grain boundary and the positioning mark by using a transmission microscope includes:
[0021] The grain boundary and the positioning mark are observed through a transmission microscope, and the point mark corresponding to the position of the grain boundary is found to complete the calibration of the position of the grain boundary.
[0022] Optionally, the using the positioning mark structure to determine the position of the grain boundary so that the center of the Josephson microbridge junction pattern in the layout is aligned with the grain boundary includes:
[0023] The reflective microscope of the ultraviolet exposure machine is used to find the dot mark for calibrating the grain boundary position, and the dot mark for calibrating the grain boundary position is aligned with the center of the Josephson microbridge junction pattern in the layout, thereby aligning the center of the Josephson microbridge junction pattern in the layout with the grain boundary.
[0024] Optionally, the size of the dot-shaped mark is 2-4 μm, and the interval between adjacent dot-shaped marks is 1-3 μm;
[0025] The size of the digital mark is 5-10 μm, and one digital mark is set every 10 dot marks;
[0026] The overall length of the Josephson microbridge junction is 8-10 μm.
[0027] Optionally, the positioning mark structure is located in a non-device area on the bicrystalline substrate and is distributed within 1 mm on both sides of the grain boundary.
[0028] Optionally, forming a micron-scale linear dot matrix positioning mark structure on the high-temperature superconducting material layer near the grain boundary includes:
[0029] forming a second photoresist layer on the high temperature superconducting material layer;
[0030] Using a layout having the positioning mark structure, patterning the second photoresist layer by exposure and development to expose a portion of the high-temperature superconducting material layer;
[0031] Depositing a metal layer on the second photoresist layer and the exposed high temperature superconducting material layer;
[0032] The second photoresist layer and the metal layer on the second photoresist layer are removed, and the remaining metal layer forms the positioning mark structure on the high-temperature superconducting material layer.
[0033] Optionally, forming a micron-scale linear dot matrix positioning mark structure on the high-temperature superconducting material layer near the grain boundary includes:
[0034] Depositing a metal layer on the high temperature superconducting material layer;
[0035] forming a third photoresist layer on the high temperature superconducting material layer;
[0036] Using a layout having the positioning mark structure, patterning the third photoresist layer by exposure and development;
[0037] Using the patterned third photoresist layer as a mask, etching the metal layer;
[0038] The third photoresist layer is removed, and the remaining metal layer forms the positioning mark structure.
[0039] Optionally, the material of the metal layer includes at least one of Ti, Cr, PdAu, Pd, and Nb;
[0040] The thickness of the metal layer is 10-50 nm.
[0041] In a second aspect, the present invention provides a high temperature superconducting quantum interference device, which is formed by the high temperature superconducting quantum interference device preparation method of accurately positioning the twin crystal junction and the grain boundary described in the first aspect.
[0042] The beneficial effects of the present invention are:
[0043] The method of the present invention prepares a micron-level, periodic positioning mark structure near the grain boundary of a twin crystal substrate on which a high-temperature superconducting thin film has been prepared, then uses a transmission microscope to find the position of the grain boundary relative to the positioning mark structure, and after forming a photoresist pattern, performs pattern alignment before exposure. Since the photoresist is transparent, a reflective microscope of an exposure machine can be used to observe and find a resolvable positioning mark structure, and a Josephson junction pattern in the layout is fixed at a positioning mark position corresponding to the calibrated grain boundary position, so that the center of the Josephson junction pattern is indirectly aligned with the grain boundary by using the positioning mark structure, and finally normal exposure and etching are performed to prepare a device. The method has a controllable and stable process and good repeatability, and can greatly improve the alignment accuracy of a small-size Josephson junction and a twin crystal substrate grain boundary.
[0044] The system of the present invention has other characteristics and advantages, which will be apparent from the drawings incorporated herein and the following detailed description, or will be described in detail in the drawings incorporated herein and the following detailed description, which together serve to explain the specific principles of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The above and other objects, features and advantages of the present invention will become more apparent through a more detailed description of exemplary embodiments of the present invention in conjunction with the accompanying drawings, in which like reference numerals generally represent like components.
[0046] Figure 1 A schematic diagram showing the DC SQUID structure.
[0047] Figure 2 A schematic diagram of a high-temperature superconducting Josephson junction formed on a bicrystalline substrate is shown.
[0048] Figure 3 A process step diagram of a method for preparing a high-temperature superconducting quantum interference device for accurately positioning a twin crystal junction and a grain boundary according to the present invention is shown.
[0049] Figure 4 The figure shows a layout of a positioning mark structure in one embodiment of the present invention.
[0050] Figure 5 A schematic diagram showing the relative positions of the positioning mark structure and the grain boundary in one embodiment of the present invention is shown.
[0051] Figure 6 A schematic diagram showing the relative positions of a Josephson microbridge junction and a positioning mark structure in an embodiment of the present invention is shown.
[0052] Figure 7 An optical microscopic structure diagram of a Josephson microbridge junction device in one embodiment of the present invention is shown. DETAILED DESCRIPTION
[0053] The present invention will be described in more detail below with reference to the accompanying drawings. Although preferred embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to make the present invention more thorough and complete, and to fully convey the scope of the present invention to those skilled in the art.
[0054] Example 1
[0055] like Figure 3 As shown, this embodiment provides a method for preparing a high-temperature superconducting quantum interference device for accurately positioning a bicrystalline junction and a grain boundary, comprising:
[0056] S1: providing a double crystal substrate, on which a high temperature superconducting material layer is deposited, and the bonding interface between the two substrates in the double crystal substrate is a grain boundary;
[0057] Specifically, the bicrystalline substrate is formed by sintering two substrates with different orientations at a certain angle, and the bonding interface of the two substrates is a grain boundary; after sintering the two substrates with different crystal orientations together, the bicrystalline substrate is also subjected to surface polishing, and then a high-temperature superconducting material layer is formed on the bicrystalline substrate through a deposition process. Optionally, the material of the bicrystalline substrate is single crystal silicon, and the material of the high-temperature superconducting material layer is yttrium barium copper oxide (YBCO), thallium barium calcium copper oxide (TBCCO) or bismuth strontium calcium copper oxide (BSCCO).
[0058] S2: forming a micrometer-scale linear dot matrix positioning mark structure on the high-temperature superconducting material layer near the grain boundary, where the straight line where the positioning mark structure is located is perpendicular to the extension direction of the grain boundary;
[0059] Specifically, Figure 4 As shown, the positioning identification structure includes multiple micrometer-level dot-shaped identifications and multiple different digital identifications; multiple dot-shaped identifications are evenly spaced along the direction perpendicular to the extension of the grain boundary, and the straight line segments where the multiple dot-shaped identifications are located intersect the grain boundary perpendicularly; multiple digital identifications are periodically distributed on one side of the multiple dot-shaped identifications along the direction perpendicular to the extension of the grain boundary, and the values of the multiple digital identifications are successively increased, such as from 1-10. Among them, the size of the dot-shaped identification is 2-4μm, preferably 3μm, and the interval between adjacent dot-shaped identifications is 1-3μm, preferably 2μm; the size of the digital identification is 5-10μm, preferably 6 microns, and a digital identification is set every 10 dot-shaped identifications to facilitate the calibration of the position of the grain boundary. The shape of the dot-shaped identification and the auxiliary identification is not limited, and can be circular, square or triangular, etc. In this embodiment, a triangle is used.
[0060] Optionally, in the positioning mark structure, an auxiliary mark ( Figure 4 The size of the auxiliary mark is preferably larger than that of the point mark to facilitate the precise location of the grain boundary.
[0061] In this step, the formed positioning mark structure is located in the non-device area (i.e., the area outside the formation of the Josephson microbridge junction) on the twin crystal substrate and is distributed within 1 mm on both sides of the grain boundary. The formation of the positioning mark structure in the non-device area will not affect the subsequent formation of the Josephson microbridge junction. At the same time, based on the approximate position of the grain boundary on the twin crystal substrate, a linear dot matrix positioning mark structure is formed within 1 mm on both sides of the grain boundary to ensure that the positioning mark structure passes through the grain boundary as a whole, so as to facilitate the subsequent use of the positioning mark structure to locate the grain boundary.
[0062] In this embodiment, a method for forming a micrometer-scale linear dot matrix positioning mark structure on a high-temperature superconducting material layer near a grain boundary includes:
[0063] depositing a metal layer on the high temperature superconducting material layer;
[0064] forming a third photoresist layer on the high temperature superconducting material layer;
[0065] Using a layout having a positioning mark structure (a mask having a positioning mark structure pattern), patterning the third photoresist layer by exposure and development;
[0066] etching the metal layer using the patterned third photoresist layer as a mask;
[0067] The third photoresist layer is removed, and the remaining metal layer forms a positioning mark structure.
[0068] The material of the metal layer includes at least one of Ti, Cr, PdAu, Pd, and Nb; the thickness of the metal layer is in the range of 10-50 nm. The metal layer can be etched by a dry etching process, such as an ion beam etching process.
[0069] In other embodiments, the method for forming a positioning mark structure may further include:
[0070] forming a second photoresist layer on the high temperature superconducting material layer;
[0071] Using a layout with a positioning mark structure, the second photoresist layer is patterned by exposure and development to expose a portion of the high-temperature superconducting material layer;
[0072] depositing a metal layer on the second photoresist layer and the exposed high temperature superconducting material layer;
[0073] The second photoresist layer and the metal layer on the second photoresist layer are removed, and the remaining metal layer forms a positioning mark structure on the high-temperature superconducting material layer.
[0074] The second photoresist layer can be removed by a wet process, such as by soaking in an acetone solution, and the unnecessary metal layer on the second photoresist layer can be removed at the same time as the second photoresist layer, and the remaining metal layer on the high-temperature superconducting material layer forms a positioning mark structure.
[0075] S3: Determine the relative position between the grain boundary and the positioning mark by transmission microscopy;
[0076] Specifically, the light source of the transmission microscope is used to illuminate the bottom of the twin-crystal substrate upward from the bottom of the transparent support platform, and the grain boundary and positioning mark are observed through the transmission microscope to find the point mark corresponding to the grain boundary position, so as to complete the calibration of the grain boundary position. Figure 5 As shown, it can be observed that the grain boundary is located near the second dot mark below the number 4 (a relatively blurred black line in the figure). The corresponding dot mark is marked for subsequent etching of the high-temperature superconducting material layer to form a Josephson microbridge junction before exposure.
[0077] S4: forming a first photoresist layer covering the high temperature superconducting material layer and the positioning mark structure;
[0078] Specifically, photoresist is spin-coated on the twin-crystal substrate to form a first photoresist layer covering the high-temperature superconducting material layer and the positioning mark structure.
[0079] S5: Using a layout with a superconducting quantum interference device structure, the position of the grain boundary is determined using a positioning mark structure, so that the center of the Josephson microbridge junction pattern in the layout is aligned with the grain boundary;
[0080] Specifically, this step uses a layout with a superconducting quantum interference device structure (a mask with a device structure pattern) to perform pattern alignment before exposure, using a reflective microscope of an ultraviolet exposure machine to find a dot mark for calibrating the position of the grain boundary through the first photoresist layer, and aligning the dot mark for calibrating the position of the grain boundary with the center of the Josephson microbridge junction pattern in the layout, thereby aligning the center of the Josephson microbridge junction pattern in the layout with the grain boundary. Figure 6 As shown, the marker structure aligned to the grain boundary is placed in the center of a Josephson microbridge junction pattern with a length of 8-10 μm.
[0081] It should be noted that photoresist is usually transparent or translucent. Therefore, even if the positioning mark structure is covered by the first photoresist layer, since the positioning mark structure (dot mark and digital mark) has a micron-level size, the positioning mark structure can be observed through the first photoresist layer through the reflective microscope of the exposure machine and the dot mark corresponding to the grain boundary can be distinguished. The positioning mark structure can be used to indirectly complete the alignment of the center of the Josephson microbridge junction pattern in the layout with the grain boundary, ensuring that the Josephson microbridge junction formed by the subsequent etching of the high-temperature superconducting material layer accurately crosses the grain boundary.
[0082] In addition, the graphics in the layout with the superconducting quantum interference device structure in this embodiment include not only the Josephson microbridge junction graphics, but also other device structure graphics connected to the Josephson microbridge junction, such as superconducting ring structure, electrode structure and other graphics.
[0083] S6: patterning the first photoresist layer by exposure and development;
[0084] Specifically, the first photoresist layer is patterned through normal exposure and development to transfer the superconducting quantum interference device structure pattern in the layout to the first photoresist.
[0085] S7: Using the patterned first photoresist layer as a mask, etching the high-temperature superconducting material layer to form a Josephson microbridge junction across the grain boundary on the twin crystal substrate to form a high-temperature superconducting quantum interference device.
[0086] Specifically, the patterned first photoresist layer is used as a mask, and preferably a dry etching process is used to etch the high-temperature superconducting material layer, and the high-temperature superconducting material layer exposed by the first photoresist layer is removed, and then the photoresist layer is removed, and the remaining high-temperature superconducting material layer forms a Josephson microbridge junction that accurately crosses the grain boundary on the bicrystalline substrate, such as Figure 7 As shown, the remaining high-temperature superconducting material layer also forms other structures such as superconducting rings and electrodes of the superconducting quantum interference device structure, and finally forms a high-temperature superconducting quantum interference device.
[0087] It can be seen that the preparation method of the high-temperature superconducting quantum interference device of the present invention is controllable and stable with good repeatability, which greatly improves the alignment accuracy of the small-sized Josephson junction and the grain boundary of the twin crystal substrate, thereby improving the production efficiency and product yield of the high-temperature superconducting quantum interference device.
[0088] Example 2
[0089] This embodiment provides a high-temperature superconducting quantum interference device, which is formed by the preparation method of the high-temperature superconducting quantum interference device of Embodiment 1.
[0090] The high-temperature superconducting quantum interference device of this embodiment is formed by the preparation method of Example 1. Since the Josephson microbridge junction is accurately crossed across the grain boundary in the manufacturing process, the high-temperature superconducting quantum interference device has a high yield rate and good product performance.
[0091] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those skilled in the art without departing from the scope and spirit of the described embodiments.
Claims
1. A method for preparing a high-temperature superconducting quantum interference device for accurately locating a twin crystal junction and a grain boundary, characterized in that: include: Providing a double crystal substrate, on which a high temperature superconducting material layer is deposited, wherein the bonding interface between two substrates in the double crystal substrate is a grain boundary; Forming a micrometer-scale linear dot matrix positioning mark structure on the high-temperature superconducting material layer near the grain boundary, wherein the straight line where the positioning mark structure is located is perpendicular to the extension direction of the grain boundary; Determining the relative position between the grain boundary and the positioning mark by a transmission microscope; forming a first photoresist layer covering the high temperature superconducting material layer and the positioning mark structure; Using a layout with a superconducting quantum interference device structure, using the positioning mark structure to determine the position of the grain boundary, so that the center of the Josephson microbridge junction pattern in the layout is aligned with the grain boundary; patterning the first photoresist layer by exposure and development; The high-temperature superconducting material layer is etched using the patterned first photoresist layer as a mask to form a Josephson microbridge junction across the grain boundary on the bicrystalline substrate to form a high-temperature superconducting quantum interference device.
2. The preparation method according to claim 1, characterized in that: The positioning mark structure includes a plurality of micrometer-level dot marks and a plurality of different digital marks; The plurality of point-shaped marks are distributed at equal intervals along a direction perpendicular to the extension direction of the grain boundary, and the straight line segment where the plurality of point-shaped marks are located intersects the grain boundary perpendicularly; The plurality of digital identifiers are periodically distributed on one side of the plurality of dot-shaped identifiers along a direction perpendicular to the extension direction of the grain boundaries, and the values of the plurality of digital identifiers are increased in sequence.
3. The preparation method according to claim 2, characterized in that: The determining the relative position between the grain boundary and the positioning mark by using a transmission microscope comprises: The grain boundary and the positioning mark are observed through a transmission microscope, and the point mark corresponding to the position of the grain boundary is found to complete the calibration of the position of the grain boundary.
4. The preparation method according to claim 3, characterized in that: The method of using the positioning mark structure to determine the position of the grain boundary so that the center of the Josephson microbridge junction pattern in the layout is aligned with the grain boundary includes: The reflective microscope of the ultraviolet exposure machine is used to find the dot mark for calibrating the grain boundary position, and the dot mark for calibrating the grain boundary position is aligned with the center of the Josephson microbridge junction pattern in the layout, thereby aligning the center of the Josephson microbridge junction pattern in the layout with the grain boundary.
5. The preparation method according to claim 2, characterized in that: The size of the dot-shaped marks is 2-4 μm, and the interval between adjacent dot-shaped marks is 1-3 μm; The size of the digital mark is 5-10 μm, and one digital mark is set every 10 dot marks; The overall length of the Josephson microbridge junction is 8-10 μm.
6. The preparation method according to claim 1, characterized in that: The positioning mark structure is located in a non-device area on the twin crystal substrate and is distributed within a range of 1 mm on both sides of the grain boundary.
7. The preparation method according to claim 1, characterized in that: The micron-scale linear dot matrix positioning mark structure is formed on the high-temperature superconducting material layer near the grain boundary, including: forming a second photoresist layer on the high temperature superconducting material layer; Using a layout having the positioning mark structure, patterning the second photoresist layer by exposure and development to expose a portion of the high-temperature superconducting material layer; Depositing a metal layer on the second photoresist layer and the exposed high temperature superconducting material layer; The second photoresist layer and the metal layer on the second photoresist layer are removed, and the remaining metal layer forms the positioning mark structure on the high-temperature superconducting material layer.
8. The preparation method according to claim 1, characterized in that: The micron-scale linear dot matrix positioning mark structure is formed on the high-temperature superconducting material layer near the grain boundary, including: Depositing a metal layer on the high temperature superconducting material layer; forming a third photoresist layer on the high temperature superconducting material layer; Using a layout having the positioning mark structure, patterning the third photoresist layer by exposure and development; Using the patterned third photoresist layer as a mask, etching the metal layer; The third photoresist layer is removed, and the remaining metal layer forms the positioning mark structure.
9. The preparation method according to claim 7 or 8, characterized in that: The material of the metal layer includes at least one of Ti, Cr, PdAu, Pd, and Nb; The thickness of the metal layer is 10-50 nm.
10. A high temperature superconducting quantum interference device, characterized in that: The high-temperature superconducting quantum interference device is formed by the high-temperature superconducting quantum interference device preparation method for accurately positioning the twin crystal junction and the grain boundary as described in any one of claims 1 to 9.
Citation Information
Cited By
Overlay alignment device and overlay alignment method for transparent bicrystal substrate covered by thin film
CN120335252A