Functionalized poly (aryl ether sulfone) copolymers

By introducing thioether functional side chain groups into poly(aryl ether sulfone) polymers to form side chain functional copolymers, the problem of insufficient hydrophilicity of PAES polymers in membrane applications is solved and the fluidity is improved. and mechanical stability, suitable for a wide range of high-performance materials and coatings.

CN118765299APending Publication Date: 2024-10-11SOLVAY SPECIALTY POLYMERS USA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280092420.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-11
Filing Date
2022-12-21
Publication Date
2024-10-11

AI Technical Summary

Technical Problem

Existing poly(aryl ether sulfone) (PAES) polymers need to adjust their hydrophilicity to improve membrane performance in certain applications, but it is difficult to effectively improve their fluidity and mechanical stability with existing technologies.

Method used

Using side chain functionalized copolymers, a new copolymer structure is formed by introducing side chain groups with thioether functional groups into the PAES polymer. The copolymer has an increased glass transition temperature and can pass The reactivity of allyl groups and carbon-carbon double bonds modulates its properties.

Benefits of technology

It is possible to improve the fluidity and biocompatibility of PAES polymer while retaining its mechanical robustness and amorphous pore structure, making it suitable for applications in membranes, composite materials and functional coatings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005006978040000022
    Figure BDA0005006978040000022
  • Figure BDA0005006978040000024
    Figure BDA0005006978040000024
  • Figure BDA0005006978040000026
    Figure BDA0005006978040000026
Patent Text Reader

Abstract

The present invention relates to side chain-functionalized poly (aryl ether sulfone) (PAES) copolymers (P1), to a process for the preparation of the copolymers (P1), and to the use thereof in the preparation of membranes, composites or coatings. The copolymer (P1) comprises PAES repeating units (RP1) and PAES side chain functionalized repeating units (R * P1).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to U.S. Provisional Patent Application No. 63 / 293106 filed on December 23, 2021 and European Patent Application No. 22161495.1 filed on March 11, 2022, the entire contents of which are incorporated by reference into this application for all purposes. Technical Field

[0003] The present disclosure relates to a side chain functionalized copolymer (P1) and a method for preparing the side chain functionalized copolymer (P1). The present invention also relates to the use of the copolymer (P1) for preparing functional membranes (i.e., hydrophobic, hydrophilic, bio-labeled fluorescently labeled membranes), the use of the copolymer (P1) in composite materials, 3D printing applications, and the use of the copolymer (P1) in functional coatings. Background Art

[0004] Poly(aryl ether sulfone) (PAES) polymers belong to the group of high-performance thermoplastics and are characterized by high heat deformation resistance, good mechanical properties, excellent hydrolysis resistance and inherent flame retardancy. Versatile and useful PAES polymers have many applications in electronics, electrical industry, medicine, general engineering, food processing and 3D printing. PAES polymers can be used in injection molded articles, composite materials and membranes (such as for water purification or hemodialysis).

[0005] PAES is typically made by polycondensation using dihalodiphenyl sulfone (sulfone monomer) and at least one aromatic diol monomer such as bisphenol A ("BPA"), diphenol ("BP"), or dihydroxydiphenyl sulfone (DHDPS), also known as bisphenol S ("BPS").

[0006] A commercially important group of PAES includes polysulfone polymers referred to herein as polysulfones, or PSUs for short. PSU polymers contain repeating units derived from the condensation of BPA and dihalosulfone monomers such as 4,4'-dichlorodiphenyl sulfone (DCDPS). Such PSU polymers are available from Solvay Specialty Polymers USA, LLC under the trademark Commercially available. The Tg of PSU is typically 185°C. The structure of the repeating unit of such a PSU polymer is shown below:

[0007]

[0008] Another important group of PAES includes polyethersulfone polymers, referred to as PES. PES polymers are derived from the condensation of BPS and dihalosulfone monomers (such as DCDPS). Such PES polymers are purchased from Solvay Specialty Polymers LLC in the United States under the trademark Commercially available. The Tg of PES is typically 220°C. The structure of the repeating unit of this PES polymer is shown below:

[0009]

[0010] Another important group of PAES includes poly(biphenyl ether sulfone) polymers, or PPSU for short. PPSU is made by reacting 4,4'-biphenol (BP) and a dihalosulfone monomer (such as DCDPS) and is notably available from Solvay Specialty Polymers LLC in the United States under the trade name Commercially available. The Tg of PPSU is typically 220°C. The structure of the repeating unit of this PPSU polymer is shown below:

[0011]

[0012] Although PAES polymers have many advantages and good physical properties, it is sometimes necessary to adjust these properties to improve performance in specific applications. For example, in membrane filtration, it is sometimes necessary to increase the hydrophilicity of PAES to improve key membrane performance attributes, such as flow rate. Modification of basic properties (including but not limited to hydrophilicity) is often achieved by combining two homopolymers to prepare block copolymers, which have a combination of the inherent properties of each individual homopolymer. For example, in membrane applications, PAES homopolymers can be covalently linked to hydrophilic homopolymers to synthesize new PAES-hydrophilic block copolymers, which have superior membrane performance due to the enhanced flow caused by the hydrophilic component, while retaining the mechanical robustness and amorphous pore structure of the PAES component.

[0013] The present invention provides a side chain functionalized copolymer and a method for preparing such copolymers. These functionalized copolymers are complex polymer structures that can be used in potentially different applications, such as for preparing membranes, composite materials and coatings. Summary of the invention

[0014] One aspect of the present disclosure relates to a side chain functionalized poly(aryl ether sulfone) (PAES) copolymer (P1) as defined in claim 1. The copolymer (P1) comprises poly(aryl ether sulfone) (PAES) repeating units (R P1 ), and a PAES repeating unit with a side group (R* P1 ), more precisely PAES repeating units functionalized with side chain groups (R* P1).

[0015] Repeating unit (R* P1 ) contains a thioether functional group which has several advantages. It is a stable but at the same time multifunctional functional group which can be easily modified to fine tune the properties of the PAES copolymer (P1).

[0016] The glass transition temperature Tg of the copolymer (P1) is equal to or greater than the glass transition temperature Tg of the copolymer (P1) composed essentially of the same repeating units (R P1 ) composed of a homopolymer Tg h , the glass transition temperature is preferably measured by differential scanning calorimetry (DSC) according to ASTM D3418. Copolymer (P1) preferably has a Tg>Tg h More preferably, Tg≥5℃+Tg h More preferably, Tg≥7℃+Tg h , and even more preferably Tg ≥ 10°C + Tg h .

[0017] The present invention also relates to a method for preparing a copolymer (P1) from a copolymer (P0) comprising allyl groups and / or functional groups containing carbon-carbon double bonds, which carbon-carbon double bonds are reactive and can therefore be used to effectively modify the copolymer. Thus, the present invention provides a method for introducing functionality into PAES polymers, and the resulting copolymers can then be further used in various applications, for example for the preparation of membranes.

[0018] The invention also relates to the use of the copolymer (P1) for preparing films, composite materials or coatings.

[0019] Disclosure of the Invention

[0020] In this application:

[0021] - even any description related to a specific embodiment is applicable to and interchangeable with other embodiments of the present disclosure;

[0022] - When an element or component is said to be included in and / or selected from a list of listed elements or components, it should be understood that in the relevant embodiments explicitly considered herein, the element or component may also be any of these listed independent elements or components, or may also be selected from a group consisting of any two or more of the explicitly listed elements or components; any element or component listed in the list of elements or components may be omitted from this list; and

[0023] - Any recitation of numerical ranges by endpoints herein includes all numbers subsumed within the recited range as well as the endpoints of that range and equivalents thereof.

[0024] In this application:

[0025] - the term "comprising" or "comprise" includes "consisting essentially of" or "consisting essentially of" as well as "consisting of" or "consisting of";

[0026] - as used herein, the singular 'a' or 'one' includes the plural unless expressly stated otherwise; and

[0027] -It should be understood that the elements, properties and / or characteristics of the (co)polymers, products or articles, methods or uses described in this specification can be explicitly or implicitly combined with other elements, properties and / or characteristics of the (co)polymers, products or articles, methods or uses in all possible ways without departing from the scope of this specification.

[0028] The term "consisting essentially of," in connection with a composition, product, article, polymer, process, method, etc., is intended to mean that any additional elements or features that may not be expressly described herein and that do not materially affect the basic and novel characteristics of such composition, product, article, polymer, process, method, etc., may be included in such an embodiment.

[0029] In the present disclosure, the term "repeating unit" refers to the smallest unit of the PAES polymer, which is repeated in the chain and is composed of the condensation of the diol compound and the dihalogenated compound. The term "recurring unit" is synonymous with the terms "repeating unit" and "structural unit".

[0030] As used herein, the term "homopolymer" encompasses polymers having only one type of repeating unit.

[0031] As used herein, the term "copolymer" encompasses polymers having two or more different types of repeating units.

[0032] Copolymer (P1)

[0033] The present invention relates to a side chain functionalized copolymer (P1). The copolymer (P1) comprises at least two types of repeating units, namely, repeating units (R) of formula (M) described below. P1 ) and a repeating unit (R*) having formula (N) P1 ). Repeating unit (R* P1 ) is functionalized with functional groups which may be selected from the group consisting of:

[0034] -(CH2) j -S-R2, wherein j is an integer from 3 to 7, and / or

[0035] -(CH2) k -CH-CH2(CH3)-S-R2, wherein k is an integer from 0 to 4,

[0036] and R2 is independently selected from the group consisting of:

[0037] -(CH2) u -COOH, wherein u is an integer from 1 to 5, preferably u is 1 or 2,

[0038] -(CH2) k -OH, wherein k is an integer from 1 to 5, preferably k is 1 or 2,

[0039] -(CH2) p -NR a R b , wherein p is an integer from 1 to 5, and a and b are independently C1-C6 alkyl or H, provided that R a and R b Cannot be all CH3; preferably -NR a R b is -NH2, and preferably p is 1 or 2,

[0040] -(CH2) q -SO3Na, wherein q is an integer from 1 to 5, preferably q is 1, 2 or 3,

[0041] -(CH2) a -COCH3, wherein a is an integer from 0 to 10,

[0042] -(CH2) r -Si(OCH3)3, wherein r is an integer from 1 to 5, preferably r is 1, 2 or 3,

[0043] -(CH2) s -(CF2) t -CF3, wherein s is an integer from 1 to 5, preferably 1 or 2, and t is an integer from 1 to 10, preferably between 5 and 9,

[0044] -C(O)-R c , where R c is C1-C6 alkyl or H, preferably H,

[0045] -(CH2)v-CH3, wherein v is an integer from 5 to 30, preferably v is an integer from 8 to 20, and

[0046] -(CH2)w-Ar, wherein w is an integer from 1 to 10, and Ar contains one or two aromatic rings or heteroaromatic rings, such as one or two benzene rings.

[0047] The functional groups of the copolymer (P1) are internal functionalizations within the copolymer backbone. The internal functionalization is produced by stepwise polymerization in the presence of an allyl-substituted monomer, which advantageously makes the system versatile, since the content of functionality can be adjusted by varying the content of allyl-substituted monomer in the reaction mixture. The allyl-substituted monomer comprises two pendant allyl side chains, each of which comprises 3 to 7 carbon atoms according to the invention.

[0048] The copolymer (P1) of the present invention comprises:

[0049] - a repeating unit (R) having the formula (M) P1 ):

[0050]

[0051] - a repeating unit (R*) having the formula (N) P1 ):

[0052]

[0053] in

[0054] - each R1 is independently selected from the group consisting of halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium;

[0055] - each i is an integer independently selected from 0 to 4;

[0056] -T is selected from the group consisting of: a bond, -CH2-; -O-; -SO2-; -S-; -C(O)-; -C(CH3)2-; -C(CF3)2-; -C(=CCl2)-; -C(CH3)(CH2CH2COOH)-; -N=N-; -R a C=CR b -, where R a and R b each independently of one another is hydrogen or C1-C12-alkyl, C1-C12-alkoxy, or C6-C18-aryl; -(CH2) m -and-(CF2) m -, wherein m is an integer from 1 to 6; a straight or branched aliphatic divalent group having up to 6 carbon atoms; and combinations thereof;

[0057] -G N Select from the following formula (GN1 ) to (G N6 ) is a group consisting of at least one of:

[0058]

[0059] Among them, in the formula (G N1 ) to (G N6 )middle,

[0060] -W is a bond or -SO2-, preferably -SO2-;

[0061] - each k is independently an integer from 0 to 4;

[0062] - each j is independently an integer from 3 to 7;

[0063] - Each R2 is independently selected from the group consisting of:

[0064] -(CH2) u -COOH, wherein u is an integer from 1 to 5, provided that when T and W are both -SO2-, then u is not 1 or 2,

[0065] -(CH2) k -OH, wherein k is an integer from 1 to 5,

[0066] -(CH2) p -NR a R b , wherein p is an integer from 1 to 5, and a and b are independently C1-C6 alkyl or H, provided that R a and R b It can't be all CH3.

[0067] -(CH2) q -SO3Na, wherein q is an integer from 1 to 5,

[0068] -(CH2) a -COCH3, wherein a is an integer from 0 to 10

[0069] -(CH2) r -Si(OCH3)3, wherein r is an integer from 1 to 5,

[0070] -(CH2) s -(CF2) t -CF3, wherein s is an integer from 1 to 5, and t is an integer from 1 to 10,

[0071] -C(O)-R c , where R c is C1-C6 alkyl or H, preferably H,

[0072] -(CH2) v -CH3, wherein v is an integer from 5 to 30, and

[0073] -(CH2) w -Ar, wherein w is an integer from 1 to 10, and Ar comprises one or two aromatic or heteroaromatic rings, such as one or two benzene rings, and wherein the glass transition temperature Tg of the copolymer (P1) is equal to or greater than that of the copolymers consisting essentially of the same repeating units (R P1 ) composed of a homopolymer Tg h , preferably Tg>Tg h , more preferably Tg≥5℃+Tg h , and more preferably Tg≥7℃+Tg h , and even more preferably Tg ≥ 10°C + Tg h The glass transition temperature is preferably measured by differential scanning calorimetry (DSC) according to ASTM D3418.

[0074] The copolymer (P1) of the present invention is in the form of a racemic product. Due to the presence of a base and high temperatures during polymerization, allyl substituted monomers usually undergo racemization during polymerization in such a way that the position of the double bond may vary along the side chain. This results in the formation of molecules that are different from each other, since the double bond may be at the end of the side chain or at a carbon before the end of the side chain. The amount of racemization depends on the reaction time and temperature.

[0075] In some embodiments, copolymer (P1) is such that in the repeating unit (R P1 ), T is selected from the group consisting of a bond, -SO2-, -C(CH3)2- and mixtures thereof. The copolymer (P1) of the present invention may, for example, comprise repeating units (R) wherein T is -C(CH3)2- P1 ) and a repeating unit in which T is -SO2- (R P1 ).

[0076] Repeating unit (R P1 ) is preferably -C(CH3)2-.

[0077] In some embodiments, copolymer (P1) is such that each R1 is independently selected from the group consisting of: C1-C12 moieties optionally containing one or more heteroatoms; sulfonic acid and sulfonate groups; phosphonic acid and phosphonate groups; amines and quaternary ammonium groups.

[0078] In some embodiments, copolymer (P1) is such that for the repeating unit (R P1 ) and repeating units (R* P1 ) for each R1,i is zero.

[0079] In some embodiments, copolymer (P1) is such that the repeating unit (R P1 ) is according to formula (M1), (M2) or (M3):

[0080]

[0081] In some embodiments, copolymer (P1) is such that it comprises:

[0082] - where group G N According to the formula (G N1 ) repeating unit (R* P1 ), preferably at least 25 mol.%, more preferably at least 30 mol.%, even more preferably 35 mol.% of the repeating unit (R* P1 ) is such that the group G N According to the formula (G N1 );

[0083] - where group G N According to the formula (G N1 ) and (G N6 ) repeating unit (R* P1 ), preferably at least 35 mol.%, more preferably at least 40 mol.%, even more preferably 45 mol.% of the repeating units (R* P1 ) is such that the group G N According to the formula (G N1 ) and (G N6 );or

[0084] - where group G N According to the formula (G N1 )、(G N4 ) and (G N6 ) of at least one repeating unit (R* P1 ), preferably at least 50 mol.%, more preferably at least 60 mol.%, even more preferably 70 mol.%, 80 mol.% or 90 mol.% of the repeating units (R* P1 ) is such that the group G N According to the formula (G N1 ) and (G N6 ).

[0085] In some embodiments, copolymer (P1) is such that in the repeating unit (R* P1 ), k is zero and j is 3.

[0086] In some embodiments, copolymer (P1) is such that in the repeating unit (R* P1 ), W is -SO2-.

[0087] In some embodiments, copolymer (P1) is such that the repeating unit (R P1 ) / repeating unit (R* P1 ) varies between 0.01 / 100 and 100 / 0.01, preferably between 1 / 100 and 100 / 1, more preferably between 1 / 1 and 12 / 1, even more preferably between 4 / 1 and 10 / 1.

[0088] In some embodiments, copolymer (P1) is such that the repeating unit (R* P1 ) wherein R2 is independently selected from the group consisting of:

[0089] -CH2-COOH,

[0090] -(CH2)2-OH,

[0091] -(CH2)2-NH2,

[0092] -(CH2)3-SO3Na,

[0093] -(CH2)3-Si(OCH3)3,

[0094] -(CH2)2-(CF2)7-CF3,

[0095] -CHO,

[0096] -(CH2)9-CH3, and

[0097] -CH2-Ph, wherein Ph is benzene.

[0098] In some embodiments, copolymer (P1) comprises at least 50 mol.% of repeating units (R P1 ) and (R* P1 ). The copolymer (P1) may, for example, comprise at least 60 mol.%, at least 70 mol.%, at least 80 mol.%, at least 90 mol.%, at least 95 mol.%, at least 99 mol.% of repeating units (R P1 ) and (R* P1 The copolymer (P1) may preferably consist essentially of repeating units (R P1 ) and (R* P1 )composition.

[0099] The glass transition temperature Tg of the PAES copolymer (P1) is preferably greater than that of the copolymer consisting essentially of the same PAES repeating units (R P1 ) composed of a homopolymer Tg h , more preferably Tg≥5℃+Tg h, more preferably Tg ≥ 7°C + Tgh, and even more preferably Tg ≥ 10°C + Tg h .

[0100] When the PAES repeating unit (R P1 ) has formula (M1) and the corresponding homopolymer is Tg h When the PSU is about 185°C, the PAES repeating unit (R P1 ) and a functionalized repeating unit (R*) having formula (N) P1 ) of a PAES copolymer (P1) (wherein in formula (G N1 ) to (G N6 ), W is a bond or -SO2-, preferably -SO2-) Tg> Tg PSU , preferably Tg≥3℃+Tg PSU , more preferably Tg≥5℃+Tg PSU , and more preferably Tg≥7℃+Tg PSU , and even more preferably Tg ≥ 10°C + Tg PSU .

[0101] When the PAES repeating unit (R P1 ) has formula (M2) and the homopolymer corresponds to Tg h When the PPSU is about 220°C, it contains the same PAES repeating unit (R P1 ) and a functionalized repeating unit (R*) having formula (N) P1 ) of a PAES copolymer (P1) (wherein in formula (G N1 ) to (G N6 ), W is a bond or -SO2-, preferably -SO2-) with a glass transition temperature Tg>Tg PPSU , preferably Tg≥3℃+Tg PPSU , more preferably Tg≥5℃+Tg PPSU , and more preferably Tg≥7℃+Tg PPSU , and even more preferably Tg ≥ 10°C + Tg PPSU .

[0102] When the PAES repeating unit (R P1 ) has formula (M3) and the homopolymer corresponds to Tg h When the PES is about 220°C, it contains the same PAES repeating unit (R P1 ) and a functionalized PAES repeating unit (R*) having formula (N) P1 ) of a PAES copolymer (P1) (wherein in formula (G N1 ) to (G N6), W is a bond or -SO2-, preferably -SO2-) Tg> Tg PES , preferably Tg≥3℃+Tg PES , more preferably Tg≥5℃+Tg PES , and more preferably Tg≥7℃+Tg PES , and even more preferably Tg ≥ 10°C + Tg PES .

[0103] This is in contrast to what is described for the functionalized PAES copolymers in WO 2020 / 187684 A1 and WO 2021 / 123405 A1, where cysteamine is used during the synthesis, where the glass transition temperature Tg of the copolymers described in the examples is less than the Tg of their corresponding homopolymers. The functionalized PSU copolymer (P1-C) of WO'684 prepared with cysteamine hydrochloride has a Tg of 175°C ( <Tg PSU The functionalized PSU copolymers (P1-A), (P1-B) and (P1-E) of WO'405 have Tg values ​​of 150°C, 143°C and 162°C ( <Tg PSU ). These functionalized PSU polymers are prepared from copolymer precursors made using DCDPS, diallyl bisphenol A and bisphenol A. The functionalized PPSU copolymer (P1-C) of WO'405 has a Tg of 170°C ( <Tg PPSU ), and the functionalized PPSU copolymer (P1-C) is prepared from a copolymer precursor made using DCDPS, diallyl bisphenol A and 4,4'-biphenol. The functionalized PES copolymer (P1-D) of WO'405 has a Tg of 190°C ( <Tg PES ), and the functionalized PES copolymer is prepared from a copolymer precursor made using DCDPS, diallyl bisphenol A and bisphenol S.

[0104] The copolymer (P1) of the present invention may have a glass transition temperature Tg ranging from 170 to 240°C or 185 to 240°C, preferably from 190 to 240°C, more preferably from 195 to 240°C or from 200 to 235°C.

[0105] The glass transition temperature is preferably measured according to ASTM D3418, preferably by differential scanning calorimetry (DSC). For example, DSC measurements can be performed using the Q100 of TA Instruments and performed under a nitrogen purge. The DSC curve is recorded by heating, cooling, reheating and then recooling the sample at a heating and cooling rate of 20°C / min between 25°C and 320°C. Unless otherwise noted, the Tg value reported is provided using the second heating curve.

[0106] Repeating unit (R*P1 ) has several advantages. First, the thioether bond is a stable, non-hydrolyzable linkage, which is important for applications in membranes, especially for medical applications. Moreover, the thioether bond is a highly biocompatible and biostable linkage, and can therefore be used in hemodialysis applications; many bioactive molecules contain thioether moieties, such as biotin. However, after treatment with a suitable oxidant (like hydrogen peroxide), this bond can be oxidized to form sulfoxide and sulfone linkages. In addition, thioethers can be easily alkylated with alkyl halides to form sulfonium salts; polymer sulfonium salts can then be used for chemical transformations, such as epoxidation. In addition, thioethers can coordinate or bond to heavy metals, so the copolymers of the present invention can be used as polymer ligands for metal removal.

[0107] The copolymers (P1) of the invention can also be characterized by their end groups. The polymer end groups are the moieties at the respective ends of the PAES copolymer (P1) chains.

[0108] Depending on the monomers used to prepare the copolymer (P0) (the copolymer (P1) is prepared from the copolymer), and the additional end-capping agent that may be used during the polycondensation process, or the protonating agent that may be added after the polymerization (in order to obtain phenol-OH end groups), the copolymer (P1) may, for example, have end groups derived from the monomers and / or end groups derived from the end-capping agent. Since the copolymer (P0) is usually manufactured by a polycondensation reaction between at least two dihydroxy components and a dihalogenated component and in the absence of an end-capping agent, the end groups of the copolymer (P1) usually include hydroxyl end groups and halogenated end groups (such as chlorinated end groups), or are preferably composed of them. The manufacture of the copolymer (P0) from which the copolymer (P1) is derived preferably excludes the use of aminophenol as an end-capping agent, which converts some halogenated end groups into amine end groups at least in part. The concentration of hydroxyl end groups can be determined by titration. The concentration of halogen groups can be determined with a halogen analyzer. However, any suitable method can be used to determine the concentration of the end groups. For example, titration, NMR, FTIR or a halogen analyzer may be used.

[0109] Process for preparing copolymer (P1)

[0110] The copolymer (P1) can be prepared by various chemical methods, for example by free radical thermal reaction, free radical UV reaction, base catalyzed reaction or nucleophilic catalyzed reaction.

[0111] The process for preparing copolymer (P1) comprises reacting an allyl / vinylidene functional copolymer (P0) with a compound having formula (I):

[0112] R2-SH, (I)

[0113] Wherein R2 is independently selected from the group consisting of:

[0114] -(CH2) u -COOH, wherein u is an integer from 1 to 5, preferably u is 1 or 2,

[0115] -(CH2) k -OH, wherein k is an integer from 1 to 5, preferably k is 1 or 2,

[0116] -(CH2) p -NR a R b , wherein p is an integer from 1 to 5, and a and b are independently C1-C6 alkyl or H, provided that R a and R b cannot all be CH3; p is preferably 1 or 2, and R a and R b Preferably CH3 or H,

[0117] -(CH2) q -SO3Na, wherein q is an integer from 1 to 5, preferably q is 1, 2 or 3,

[0118] -(CH2) a -COCH3, wherein a is an integer from 0 to 10,

[0119] -(CH2) r -Si(OCH3)3, wherein r is an integer from 1 to 5, preferably r is 1, 2 or 3,

[0120] -(CH2) s -(CF2) t -CF3, wherein s is an integer from 1 to 5, preferably 1 or 2, and t is an integer from 1 to 10, preferably 5 to 9, and

[0121] -C(O)-R c , where R c is C1-C6 alkyl or H, preferably H,

[0122] -(CH2) v -CH3, wherein v is an integer from 5 to 30, preferably v is selected from 8 to 20, and

[0123] -(CH2) w -Ar, wherein w is an integer from 1 to 10, and Ar contains one or two aromatic rings or heteroaromatic rings, such as one or two benzene rings.

[0124] The copolymer (P0) used in the process of the invention comprises repeating units (R*) having two pendant allyl / vinylidene side chains. P0), these repeating units are reactive with the compound R2-SH. The copolymer (P0) more specifically comprises:

[0125] - a repeating unit (R) having the formula (M) P0 ):

[0126]

[0127] - a repeating unit (R*) having formula (P) P0 ):

[0128]

[0129] in

[0130] - each R1 is independently selected from the group consisting of halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium;

[0131] - each i is independently selected from 0 to 4;

[0132] -T is selected from the group consisting of: a bond, -CH2-; -O-; -SO2-; -S-; -C(O)-; -C(CH3)2-; -C(CF3)2-; -C(=CCl2)-; -C(CH3)(CH2CH2COOH)-; -N=N-; -R a C=CR b -, where R a and R b each independently of one another is hydrogen or C1-C12-alkyl, C1-C12-alkoxy, or C6-C18-aryl; -(CH2) m -and-(CF2) m -, wherein m is an integer from 1 to 6; a straight or branched aliphatic divalent group having up to 6 carbon atoms; and combinations thereof,

[0133] -G p Select from the following formula (G P1 ) to (G P3 ) is a group consisting of at least one of:

[0134]

[0135] in:

[0136] -W is a bond or -SO2-, preferably -SO2-;

[0137] - Each k is independently an integer from 0 to 4.

[0138] When T and W are both -SO2-, then u is not equal to 1 or 2.

[0139] In some embodiments, the copolymer (P0) is such that in the repeating unit (R* P0 ), k is zero.

[0140] The reaction for preparing copolymer (P1) is preferably carried out in a solvent. When the reaction for preparing copolymer (P1) is carried out in a solvent, the solvent is, for example, a polar aprotic solvent selected from the group consisting of: N-methylpyrrolidone (NMP), N-butylpyrrolidone (NBP), N-ethyl-2-pyrrolidone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), 1,3-dimethyl-2-imidazolidinone, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), chlorobenzene, anisole and sulfolane. The solvent can also be chloroform or dichloromethane (DCM). The reaction for preparing copolymer (P1) is preferably carried out in sulfolane or NMP.

[0141] The molar ratio of compound of formula (I) / polymer (P0) may vary between 0.01 / 100 and 100 / 0.01, preferably between 1 / 100 and 100 / 1, more preferably between 1 / 1 and 10 / 1.

[0142] The temperature of the reaction for preparing copolymer (P1) varies between 10 and 300 °C, preferably between room temperature and 200 °C, or more preferably between 35 and 100 °C.

[0143] In some embodiments, the copolymer (P0) is such that the repeating unit (R P0 ) wherein T is selected from the group consisting of a bond, -SO2-, -C(CH3)2- and any mixture thereof. The copolymer (P0) may, for example, comprise repeating units (R) wherein T is -C(CH3)2- P0 ) and a repeating unit in which T is -SO2- (R P1 ).

[0144] Repeating unit (R P0 ) is preferably -C(CH3)2-.

[0145] In some embodiments, copolymer (P0) is such that each R1 is independently selected from the group consisting of: a C1-C12 moiety optionally comprising one or more heteroatoms; sulfonic acid and sulfonate groups; phosphonic acid and phosphonate groups; amines and quaternary ammonium groups.

[0146] In some embodiments, the copolymer (P0) is such that for the repeating unit (R P0 ) and repeating units (R* P0) for each R1,i is zero.

[0147] In some embodiments, the copolymer (P0) is such that in the repeating unit (R P0 ), j is 2.

[0148] In some embodiments, the copolymer (P0) is such that the repeating unit (R P0 ) / repeating unit (R* P0 ) varies between 0.01 / 100 and 100 / 0.01, preferably between 1 / 100 and 100 / 1.

[0149] In some embodiments, the copolymer (P0) is such that the repeating unit (R P0 ) is according to formula (M1), (M2) or (M3):

[0150]

[0151]

[0152] In some embodiments, copolymer (P0) comprises at least 50 mol.% of repeating units (R P0 ) and (R* P0 The copolymer (P0) may, for example, contain at least 60 mol%, at least 70 mol%, at least 80 mol%, at least 90 mol%, at least 95 mol%, at least 99 mol% of repeating units (R P0 ) and (R* P0 The copolymer (P0) preferably consists essentially of repeating units (R P0 ) and (R* P0 )composition.

[0153] The glass transition temperature Tg of the copolymer (P0) is equal to or greater than that of the copolymers composed essentially of the same repeating units (R P0 ) composed of a homopolymer Tg h , preferably Tg>Tgh, more preferably Tg≥5°C+Tgh, yet more preferably Tg≥7°C+Tgh, yet even more preferably Tg≥10°C+Tgh, the glass transition temperature is preferably measured by differential scanning calorimetry (DSC) according to ASTM D3418.

[0154] This is in contrast to that described for the functionalized PAES copolymers in WO 2020 / 187684 A1 and WO 2021 / 123405 A1, where cysteamine was used during synthesis, and the Tg of the copolymer (P0) described in their examples was less than the Tg of its corresponding homopolymer. The allyl / vinylidene-modified PSU copolymer (P0-A) of WO’684 has a Tg of 175 °C (<TgPSU). The allyl / vinylidene-modified PSU copolymers (P0-A) and (P0-B) of WO’405 have Tgs of 160.5 °C and 154 °C (<TgPSU), and these copolymer precursors were made using DCDPS, diallyl bisphenol A, and bisphenol A. The allyl / vinylidene-modified PPSU copolymer (P0-C) of WO’405 has a Tg of 179 °C (<TgPPSU), and this copolymer precursor (P0-C) was made using DCDPS, diallyl bisphenol A, and 4,4'-biphenol. The allyl / vinylidene-modified PES copolymer (P0-D) of WO’405 has a Tg of 187 °C (<Tg PES ), and this copolymer precursor (P0-D) was made using DCDPS, diallyl bisphenol A, and bisphenol S.

[0155] According to the examples, the copolymer (P0) of the present invention can have a Tg in the range of 170 °C to 240 °C, preferably 180 °C to 240 °C or 185 °C to 240 °C, more preferably 190 °C to 240 °C, still more preferably 195 °C to 240 °C or 195 °C to 235 °C, and the Tg is measured by DSC as described herein.

[0156] In some embodiments, the compound R2-SH used to react with the copolymer (P0) is such that R2 in the repeating unit (R* P1 ) is independently selected from the group consisting of:

[0157] -CH2-COOH,

[0158] -(CH2)2-OH,

[0159] -(CH2)2-NH2,

[0160] -(CH2)3-SO3Na,

[0161] -(CH2)3-Si(OCH3)3,

[0162] -(CH2)2-(CF2)7-CF3,

[0163] -CHO,

[0164] -(CH2)9-CH3, and

[0165] -CH2-Ph, wherein Ph is benzene.

[0166] In some embodiments, the reaction for preparing copolymer (P1) can be carried out in the presence of a base, for example, selected from the group consisting of potassium carbonate (K2CO3), potassium tert-butoxide, sodium hydroxide (NaOH), potassium hydroxide (KOH), sodium carbonate (Na2CO3), cesium carbonate (Cs2CO3) and sodium tert-butoxide. The base can also be selected from the group consisting of N-ethyl-N-(propan-2-yl) propan-2-amine (Hunig base), triethylamine (TEA) and pyridine.

[0167] In some embodiments, the reaction used to prepare copolymer (P1) can be carried out in the presence of:

[0168] - at least one free radical initiator, preferably 2,2'-azobis(2-methylpropionitrile) (AIBN), and / or

[0169] - At least one catalyst, preferably chosen from peroxides and hydroperoxides.

[0170] According to an embodiment, the amount of copolymer (P1) at the end of the reaction is at least 10 wt.%, eg at least 15 wt.%, at least 20 wt.% or at least 30 wt.%, based on the total weight of copolymer (P0) and solvent.

[0171] At the end of the reaction, the copolymer (P1) is separated from the other components (salt, base, ...) to obtain a solution. Filtration can be used, for example, to separate the copolymer (P1) from the other components. The solution can then be used as is to react the copolymer (P1) with other compounds, or alternatively, the copolymer (P1) can be recovered from the solvent, for example, by condensation or devolatilization of the solvent.

[0172] Method for preparing copolymer (P0)

[0173] In some embodiments, the allyl / vinylidene functionalized copolymer (P0) used in the method of the present invention is prepared by condensation of at least one aromatic dihydroxy monomer (a1) with at least one aromatic sulfone monomer (a2) comprising at least two halogen substituents and at least one allyl-substituted aromatic dihydroxy monomer (a3).

[0174] The condensation for preparing the copolymer (P0) is preferably carried out in a solvent. When the condensation for preparing the copolymer (P0) is carried out in a solvent, the solvent is, for example, a polar aprotic solvent selected from the group consisting of: N-methylpyrrolidone (NMP), N-butylpyrrolidone (NBP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), 1,3-dimethyl-2-imidazolidinone, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), chlorobenzene and sulfolane. The condensation for preparing the copolymer (P0) is preferably carried out in sulfolane or NMP.

[0175] The condensation for preparing copolymer (P0) can be carried out in the presence of a base, for example selected from the group consisting of potassium carbonate (K2CO3), potassium tert-butoxide, sodium hydroxide (NaOH), potassium hydroxide (KOH), sodium carbonate (Na2CO3), cesium carbonate (Cs2CO3) and sodium tert-butoxide. The base is used to deprotonate components (a1) and (a3) ​​during the condensation reaction.

[0176] The molar ratio (a1)+(a3) / (a2) may be 0.9 to 1.1, for example 0.92 to 1.08, or 0.95 to 1.05.

[0177] In some embodiments, monomer (a2) is a 4,4-dihalosulfone comprising at least one of 4,4'-dichlorodiphenyl sulfone (DCDPS) or 4,4'difluorodiphenyl sulfone (DFDPS), preferably DCDPS.

[0178] In some embodiments, monomer (a1) comprises at least 50 wt.% of 4,4'-dihydroxybiphenyl (biphenol), at least 50 wt.% of 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), or at least 50 wt.% of 4,4'-dihydroxydiphenyl sulfone (bisphenol S), based on the total weight of monomer (a1).

[0179] In some embodiments, monomer (a3) ​​comprises at least 50 wt. % of 2,2'-diallylbisphenol A (DABA) based on the total weight of monomer (a1).

[0180] According to the condensation used to prepare the copolymer (P0), the monomers of the reaction mixture are usually reacted simultaneously. The reaction is preferably carried out in one stage. This means that the deprotonation of monomers (a1) and (a3) ​​and the condensation reaction between monomers (a1) / (a3) and (a2) occur in a single reaction stage without separation of intermediate products.

[0181] According to an embodiment, the condensation is carried out in a mixture of a polar aprotic solvent and a solvent that forms an azeotropic mixture with water. The solvent that forms an azeotropic mixture with water includes aromatic hydrocarbons, such as benzene, toluene, xylene, ethylbenzene, chlorobenzene, etc. It is preferably toluene or chlorobenzene. The solvent that forms an azeotropic mixture and the polar aprotic solvent are typically used in a weight ratio of about 1:10 to about 1:1, preferably about 1:5 to about 1:1. Water is continuously removed from the reaction material as an azeotropic mixture with a solvent that forms an azeotropic mixture, so that a substantially anhydrous condition is maintained during polymerization. After removing the water formed in the reaction, the solvent that forms an azeotropic mixture (e.g., chlorobenzene) is typically removed from the reaction mixture by distillation, so that the copolymer (P0) is dissolved in the polar aprotic solvent.

[0182] The temperature of the reaction mixture used to prepare the copolymer (P0) is maintained at about 150°C to about 350°C, preferably about 210°C to about 300°C for about 1 hour to 15 hours.

[0183] Before or after isolation of the copolymer (P0), inorganic components (eg sodium chloride or potassium chloride or excess alkali) may be removed by suitable methods such as dissolution and filtration, sieving or extraction.

[0184] According to an embodiment, the amount of copolymer (P0) at the end of the condensation is at least 30 wt.%, for example at least 35 wt.%, or at least 37 wt.%, or at least 40 wt.%, based on the total weight of copolymer (P0) and polar aprotic solvent.

[0185] At the end of the reaction, the copolymer (P0) is separated from the other components (salt, alkali, ...) to obtain a solution. Filtration can be used, for example, to separate the copolymer (P0) from the other components. The solution can then be used as is in the method of the invention to react the copolymer (P0) with the compound R2-SH, or alternatively, the copolymer (P0) can be recovered from the solvent, for example, by condensation or devolatilization of the solvent.

[0186] application

[0187] The copolymers (P1) of the present invention can be used to prepare functional membranes. For example, these membranes can be hydrophobic, hydrophilic, biolabeled, for example, membranes with fluorescent labels.

[0188] The copolymers (P1) of the invention can also be used to prepare composite materials. In this application, the functionality improves the adhesion of the resin to the reinforcing fibers, thereby improving the properties.

[0189] The copolymers (P1) of the present invention can also be used to prepare functional coatings. The chemical moieties on the surface of the coating can be selected to make the coating hydrophobic, hydrophilic, biomarkable, antimicrobial, antifouling and / or UV curable.

[0190] Should the disclosure of any patents, patent applications, and publications incorporated by reference into this application conflict with the description of this application to the extent that a term may be unclear, this description shall take precedence.

[0191] The present invention will now be described in more detail with reference to the following examples, the purpose of which is merely illustrative and not limiting the scope of the present invention.

[0192] Examples

[0193] raw materials

[0194] DCDPS (4,4'-dichlorodiphenyl sulfone), available from Solvay Specialty Polymers

[0195] BPA (Bisphenol A), available from Covestro, USA

[0196] BP (biphenol), polymer grade, available from Honshu Chemicals, Japan

[0197] daBPA-S (2,2'-diallylbisphenol S), available from Toronto Research Chemicals.

[0198] K2CO3 (potassium carbonate), available from Armand Products

[0199] NMP (2-methylpyrrolidone), available from Sigma-Aldrich, USA

[0200] MCB (methyl chlorobenzene), available from Sigma-Aldrich, USA

[0201] ADVN (2,2'-azobis(2,4-dimethylvaleronitrile)), available from Miller-Stephenson Chemical Co., Inc.

[0202] AIBN (2,2-azobis(2-methylpropionitrile)), available from Sigma-Aldrich, USA

[0203] Test Method

[0204] GPC-Molecular weight (Mn, Mw)

[0205] Method 1: Methylene chloride was used as the mobile phase for measuring molecular weight by gel permeation chromatography (GPC). Two 5 μ mixed D columns with guard columns from Agilent Technologies were used for separation. A 254 nm UV detector was used to obtain a chromatogram. A flow rate of 1.5 mL / min and an injection volume of 0.2 w / v% solution of 20 μ L in the mobile phase were selected. Calibration was performed with 12 narrow molecular weight polystyrene standards (peak molecular weight range: 371,000 to 580 g / mol). Number average molecular weight Mn, weight average molecular weight Mw, and higher average molecular weight Mz were reported.

[0206] Method 2: Viscotek GPC Max (autosampler, pump and degasser) with TDA302 triple detector array consisting of RALS (right angle light scattering), RI and viscosity detector was used. The sample was run at 1.0 mL / min through a set of 3 columns in NMP containing 0.2 w / w% LiBr at 65°C: guard column (CLM1019-with 20k Da exclusion limit), high Mw column (CLM1013, 10 MM Daltons relative to polystyrene exclusion) and low Mw column (CLM1011-20k Daltons relative to PS exclusion limit). Calibration was completed using a single monodisperse polystyrene standard of about 100 k Da. Light scattering, RI and viscosity detectors were calibrated based on a set of input data provided according to the standard. The sample was prepared in NMP / LiBr at about 2 mg / mL.

[0207] Viscotek's OMNISec v4.6.1 software was used for data analysis. Number average molecular weight Mn, weight average molecular weight Mw, and higher average molecular weight Mz are reported.

[0208] Thermogravimetric analysis (TGA)

[0209] TGA experiments were performed using a TGA Q500 from TA Instruments. TGA measurements were obtained by heating the sample from 20°C to 800°C at a heating rate of 10°C / min under nitrogen.

[0210] 1 H NMR

[0211] Measured using a 400 MHz Bruker spectrometer with TCE or DMSO as the deuterated solvent 1 H NMR spectroscopy. All spectra are referenced to residual protons in the solvent.

[0212] DSC

[0213] DSC was used to determine the glass transition temperature (Tg) and melting point (Tm) (if present). DSC experiments were performed using the Q100 of TA Instruments. The DSC curve was recorded by heating, cooling, reheating and then recooling the sample at a heating and cooling rate of 20°C / min between 25°C and 320°C. All DSC measurements were taken under nitrogen purge. Unless otherwise noted, the Tg (and Tm, if any) values ​​reported were provided using the second heating curve.

[0214] I. Preparation of copolymer (PO-A)

[0215] Copolymer (P0-A) was prepared according to Scheme 1.

[0216] The polymerization was carried out in a glass reactor vessel (1 L) equipped with an overhead stirrer, a nitrogen inlet and an overhead distillation apparatus. First, monomer 4,4'-dichlorodiphenyl sulfone (143.58 g), bisphenol A (102.73 g) and 2,2'diallyl bisphenol S (16.52 g) were added to the container, followed by potassium carbonate (78.29 g) and NMP (690 g) and chlorobenzene (170 g). The reaction mixture was heated from room temperature to 190 ° C using a heating ramp of 150 ° C / min, and chlorobenzene was continuously removed using a Dean-Stark device. Depending on the viscosity of the solution, the temperature of the reaction mixture was maintained for about eight hours. The reaction was stopped by turning off the heat source and diluting the reaction mixture with a cold solvent. The reaction mixture was filtered, condensed in methanol and dried at 110 ° C.

[0217] Characterization of copolymer (P0-A)

[0218] GPC (method 1): Mn = 12743 g / mol, Mw = 58832 g / mol, PDI = 4.61

[0219] TGA: 477℃; DSC: Tg=195℃

[0220] 1 H NMR: The presence of unsaturated groups was confirmed by the appearance of multiple peaks at 6.1-6.4 ppm, indicating that 2,2'-diallyl BPS monomers were incorporated into the polymer.

[0221] II. Preparation of copolymer (P0-B)

[0222] Copolymer (P0-B) was prepared according to Scheme 2.

[0223] The polymerization was carried out in a glass reactor vessel (1 L) equipped with an overhead stirrer, a nitrogen inlet and an overhead distillation apparatus. First, monomers 4,4'-dichlorodiphenyl sulfone (172.29 g), 4,4'-biphenol (106.13 g) and 2,2'-diallyl bisphenol S (9.91 g) were added to the container, followed by potassium carbonate (93.69 g) and cyclopentane (570 g). The reaction mixture was heated from room temperature to 210 ° C using a heating ramp of 150 ° C / min. The temperature of the reaction mixture was maintained for about five hours depending on the viscosity of the solution. The reaction was stopped by removing the heat source and diluting with more solvent. The reaction mixture was filtered, condensed in methanol and dried at 110 ° C.

[0224] Characterization of copolymer (P0-B)

[0225] GPC (method 1): Mn = 19251 g / mol, Mw = 71960 g / mol, PDI = 3.70.

[0226] TGA: 505℃; DSC: Tg=235℃

[0227] 1 H NMR: No spectra were obtained due to poor solubility in NMR solvents.

[0228] III. Preparation of functionalized copolymers (P1-A) by free radical reaction

[0229] According to Scheme 3, the copolymer (P1-A) according to the invention is prepared.

[0230] In a 250 mL three-necked flask equipped with a nitrogen inlet, a thermocouple and an overhead stirrer, 31.2 g of copolymer (PO-A) prepared according to Part I (Scheme 1) above was dissolved in 89 g of NMP and 3.2 g of cysteamine hydrochloride was added. The reaction mixture was heated to 50° C. under nitrogen and then 0.8 g of ADVN was added in one portion. The reaction was continued for 24 hours after which the reaction mass was coagulated in methanol and the precipitated polymer was then washed with methanol, water, and then finally with methanol and dried under reduced pressure at 110° C.

[0231] Characterization

[0232] GPC (method 2): Mw = 152023 g / mol, Mn = 50044 g / mol, PDI = 3.30

[0233] DSC: Tg=206℃; TGA: 411℃

[0234] A quantitative estimate of the amine functionalization was analyzed by titration of the amine groups. Amine content: 295 microequivalents / g.

[0235] Preparation of functionalized copolymers (P1-B) by free radical reaction

[0236] According to Scheme 4, the copolymer (P1-B) according to the invention is prepared.

[0237] In a 250 mL three-necked flask equipped with a nitrogen inlet, a thermocouple and an overhead stirrer, 30 g of copolymer (PO-B) prepared according to Part II (Scheme 2) above was dissolved in 110 g of NMP and 3.9 g of sodium 3-mercapto-1-propanesulfonate was added. The reaction mixture was heated to 75° C. under nitrogen and 0.59 g of AIBN was then added in one go. The reaction was continued for 24 hours, after which the reaction mass was coagulated in methanol, the precipitated polymer was then washed with methanol, water, and then finally with methanol, and dried under reduced pressure at 110° C.

[0238] Characterization

[0239] GPC (method 2): Mw = 342287 g / mol, Mn = 75154 g / mol, PDI = 4.50

[0240] DSC: Tg=234℃; TGA: 517℃

[0241] Sodium content: 1337ppm

[0242]

[0243]

[0244]

Claims

1. A copolymer (P1), comprising: - a repeating unit (R) having the formula (M) P1 ): - a repeating unit (R*) having the formula (N) P1 ): in - each R1 is independently selected from the group consisting of halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium; - each i is independently an integer from 0 to 4; -T is selected from the group consisting of: a bond, -CH2-; -O-; -SO2-; -S-; -C(O)-; -C(CH3)2-; -C(CF3)2-; -C(=CCl2)-; -C(CH3)(CH2CH2COOH)-; -N=N-; -R a C=CR b -, where R a and R b are each independently hydrogen or C1-C12-alkyl, C1-C12-alkoxy, or C6-C18-aryl; -(CH2) m -and-(CF2) m -, wherein m is an integer from 1 to 6; a straight or branched aliphatic divalent group having up to 6 carbon atoms; and combinations thereof; -G N Select from the following formula (G N1 ) to (G N6 ) is a group consisting of at least one of: in -W is a bond or -SO2-, preferably -SO2-; - each k is independently an integer from 0 to 4; - each j is independently an integer from 3 to 7; - Each R2 is independently selected from the group consisting of: -(CH2) u -COOH, wherein u is an integer from 1 to 5, provided that when T and W are both -SO2-, then u is not 1 or 2, -(CH2) k -OH, wherein k is an integer from 1 to 5, -(CH2) p -NR a R b , wherein p is an integer from 1 to 5, and a and b are independently C1-C6 alkyl or H, provided that R a and R b It can't be all CH3. -(CH2) q -SO3Na, wherein q is an integer from 1 to 5, -(CH2) a -COCH3, wherein a is an integer from 0 to 10 -(CH2) r -Si(OCH3)3, wherein r is an integer from 1 to 5, -(CH2) s -(CF2) t -CF3, wherein s is an integer from 1 to 5, and t is an integer from 1 to 10, -C(O)-R c , where R c is C1-C6 alkyl or H, preferably H, -(CH2) v -CH3, wherein v is an integer from 5 to 30, and -(CH2) w -Ar, wherein w is an integer from 1 to 10, and Ar contains one or two aromatic rings or heteroaromatic rings, such as one or two benzene rings; and The glass transition temperature Tg of the copolymer (P1) is equal to or greater than the glass transition temperature Tg of the copolymer (P1) which is substantially composed of the same repeating units (R P1 ) composed of a homopolymer Tg h , the glass transition temperature is measured by differential scanning calorimetry (DSC).

2. The copolymer (P1) according to claim 1, wherein Repeating unit (R P1 ) is selected from the group consisting of a bond, -SO2- and -C(CH3)2-.

3. The copolymer (P1) according to any one of claims 1 to 2, wherein For the repeating unit (R P1 ) and repeating units (R* P1 ) for each R1,i is zero.

4. The copolymer (P1) according to any one of claims 1 to 3, wherein In the repeating unit (R* P1 ), k is 0 and j is 3.

5. The copolymer (P1) according to any one of claims 1 to 4, wherein Repeating unit (R P1 ) / repeating unit (R* P1 ) varies between 0.01 / 100 and 100 / 0.01, preferably between 1 / 100 and 100 / 1, more preferably between 1 / 1 and 10 / 1.

6. The copolymer (P1) according to any one of claims 1 to 5, wherein Repeating unit (R P1 ) is according to formula (M1), (M2) or (M3):

7. The copolymer (P1) according to any one of claims 1 to 6, wherein Formula (G N1 )、(G N2 )、(G N3 )、(G N4 )、(G N5 ) or (G N6 ) wherein R2 is independently selected from the group consisting of: -CH2-COOH, -(CH2)2-OH, -(CH2)2-NH2, -(CH2)3-SO3Na, -(CH2)3-Si(OCH3)3, -(CH2)2-(CF2)7-CF3, -CHO, -(CH2)9-CH3, -CH2-Ph, wherein Ph is benzene.

8. The copolymer (P1) according to any one of claims 1 to 7, comprising at least 50 mol.% of repeating units (R P1 ) and (R* P1 ).

9. A method for preparing a copolymer (P1) as claimed in any one of claims 1 to 8, comprising reacting the following two substances in a solvent: a copolymer (P0) comprising - a repeating unit (R) having the formula (M) P0 ): - a repeating unit (R*) having formula (P) P0 ): in - each R1 is independently selected from the group consisting of halogen, alkyl, alkenyl, alkynyl, aryl, ether, thioether, carboxylic acid, ester, amide, imide, alkali metal or alkaline earth metal sulfonate, alkyl sulfonate, alkali metal or alkaline earth metal phosphonate, alkyl phosphonate, amine and quaternary ammonium; - each i is independently an integer from 0 to 4; -T is selected from the group consisting of: a bond, -CH2-; -O-; -SO2-; -S-; -C(O)-; -C(CH3)2-; -C(CF3)2-; -C(=CCl2)-; -C(CH3)(CH2CH2COOH)-; -N=N-; -R a C=CR b -, where R a and R b each independently of one another is hydrogen or C1-C12-alkyl, C1-C12-alkoxy, or C6-C18-aryl; -(CH2) m -and-(CF2) m -, wherein m is an integer from 1 to 6; a straight or branched aliphatic divalent group having up to 6 carbon atoms; and combinations thereof, -G p Select from the following formula (G p1 ) to (G p3 ) is a group consisting of at least one of: in: -W is a bond or -SO2-, preferably -SO2-; - each k is independently selected from 0 to 4, The glass transition temperature Tg of the copolymer (P0) is equal to or greater than the glass transition temperature Tg of the copolymer (P0) which is substantially composed of the same repeating units (R P0 ) composed of a homopolymer Tg h , preferably Tg>Tg h , more preferably Tg≥5℃+Tg h , and more preferably Tg≥7℃+Tg h , and even more preferably Tg ≥ 10°C + Tg h , the glass transition temperature is measured by differential scanning calorimetry (DSC), Compounds having formula (I): R2-SH(I) Wherein R2 is selected from the group consisting of: -(CH2) u -COOH, wherein u is an integer from 1 to 5, provided that when T and W are both -SO2-, then u is not 1 or 2, -(CH2) k -OH, wherein k is an integer from 1 to 5, -(CH2) p -NR a R b , wherein p is an integer from 1 to 5, and a and b are independently C1-C6 alkyl or H, provided that R a and R b It can't be all CH3. -(CH2) q -SO3Na, wherein q is an integer from 1 to 5, -(CH2) a -COCH3, wherein a is an integer from 0 to 10 -(CH2) r -Si(OCH3)3, wherein r is an integer from 1 to 5, -(CH2) s -(CF2) t -CF3, wherein s is an integer from 1 to 5, and t is an integer from 1 to 10, -C(O)-R c , where R c is C1-C6 alkyl or H, -(CH2) v -CH3, wherein v is an integer from 5 to 30, and -(CH2) w -Ar, wherein w is an integer from 1 to 10, and Ar contains one or two aromatic rings or heteroaromatic rings, Wherein the molar ratio of compound (I) / polymer (P0) varies between 0.01 / 100 and 100 / 0.01, the reaction is carried out at a temperature ranging from 10°C to 300°C.

10. The method of claim 9, which is carried out in a solvent selected from the group consisting of N-methylpyrrolidone (NMP), N-butylpyrrolidone (NBP), N-ethyl-2-pyrrolidone, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), 1,3-dimethyl-2-imidazolidinone, tetrahydrofuran (THF), dimethyl sulfoxide (DMSO), chlorobenzene, anisole, chloroform, dichloromethane (DCM) and sulfolane.

11. The method of any one of claims 9-10, carried out in the presence of: - at least one free radical initiator, preferably 2,2'-azobis(2-methylpropionitrile) (AIBN), and / or - at least one catalyst, preferably chosen from peroxides and hydroperoxides, and / or - in the presence of a base, preferably selected from the group consisting of N-ethyl-N-(propan-2-yl)propan-2-amine (Hennig's base), triethylamine (TEA) and pyridine.

12. The method according to any one of claims 9-10, which is carried out by exposing the reaction mixture to UV light at a wavelength in the range of 300 nm to 600 nm, preferably 350 nm to 450 nm, more preferably 365 nm.

13. The method according to any one of claims 9 to 12, wherein: The functionalized PAES copolymer (P0) comprises at least 50 mol.% of repeating units (R P0 ) and (R* P0 ).

14. The method according to any one of claims 9 to 13, wherein: The functionalized PAES copolymer (P0) is prepared by condensation of at least one aromatic dihydroxy monomer (a1) with at least one aromatic sulfone monomer (a2) containing at least two halogen substituents and at least one allyl-substituted aromatic dihydroxy monomer (a3).

15. Use of a copolymer (P1) as claimed in any one of claims 1 to 8 for the preparation of films, composite materials or coatings.