Electrochemical device
By doping anions in the positive active material of the electrochemical device and setting up a carbon layer to optimize the pore distribution, the problem of reduced characteristics of the electrochemical device at low temperatures is solved, and the high and low temperature characteristics and drift characteristics are improved.
Patent Information
- Application Number
- CN202380023812.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-28
- Filing Date
- 2023-02-15
- Publication Date
- 2024-10-11
AI Technical Summary
Existing electrochemical devices exhibit problems with reduced low-temperature characteristics and drift characteristics under low-temperature conditions. In particular, the hydrophobicity of conductive polymers causes an increase in internal resistance of the electrode, affecting electrochemical performance.
By doping anions into the positive active material and setting up a carbon layer in the electrode structure, the pore distribution is optimized so that the volume ratio V1/V0 of pore diameters below 0.2 μm reaches above 0.40, thereby improving conductivity and reducing internal resistance. .
It achieves high and low temperature characteristics and drift characteristics under low temperature conditions, improves the voltage and capacitance performance of the electrochemical device, and significantly reduces the internal resistance.
Smart Images

Figure CN118765431A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an electrochemical device. Background Art
[0002] In recent years, electrochemical devices having an intermediate structure between lithium-ion secondary batteries and electric double layer capacitors have attracted attention.
[0003] Patent document 1 (International Publication No. 2020 / 067169) discloses "an electrochemical device comprising a pair of electrodes and an electrolyte, wherein at least one of the pair of electrodes comprises an electrode collector and an electrode material layer supported on the electrode collector, wherein the electrode material layer comprises at least a conductive polymer, and the log differential pore volume distribution of the electrode material layer has at least one peak in a range of pore diameters of 50 nm or more."
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: International Publication No. 2020 / 067169 Summary of the invention
[0007] Problems to be solved by the invention
[0008] Currently, electrochemical devices having an intermediate structure between lithium ion secondary batteries and electric double layer capacitors are required to have improved characteristics at low temperatures. One object of the present disclosure is to provide an electrochemical device having high low temperature characteristics.
[0009] Means for solving problems
[0010] One aspect of the present disclosure relates to an electrochemical device. The electrochemical device includes a positive electrode, a negative electrode, and a lithium ion conductive electrolyte, wherein the positive electrode includes a positive electrode mixture layer containing a positive electrode active material, the positive electrode active material includes particles of a conductive polymer that can be reversibly doped and dedoped with anions, and when the pore distribution of the positive electrode is measured using a mercury porosimeter, a ratio V1 / V0 of a volume V1 of pores with a pore diameter of 0.2 μm or less to a volume V0 of all pores is 0.40 or more.
[0011] Effects of the Invention
[0012] According to the present disclosure, an electrochemical device with excellent low-temperature characteristics can be obtained.
[0013] Although the novel features of the present invention are described in the appended claims, both aspects of the present invention regarding the configuration and content together with other objects and features of the present invention should be more fully understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a cross-sectional view schematically showing the structure of an example of the electrochemical device according to the present embodiment.
[0015] Figure 2 It is schematically shown Figure 1 FIG. 1 is a partially exploded perspective view of an example of an electrode group of an electrochemical device shown. DETAILED DESCRIPTION
[0016] Hereinafter, the embodiments of the electrochemical device of the present disclosure are described with examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values and materials are sometimes illustrated, but other numerical values and materials may also be applied as long as the effects of the present disclosure can be obtained. In this specification, the description of "numerical value A to numerical value B" includes numerical value A and numerical value B, and can be read as "numerical value A or above and numerical value B or below". In the following description, when the lower limit and upper limit of the numerical value of a specific physical property, condition, etc. are illustrated, as long as the lower limit is not above the upper limit, any of the illustrated lower limits can be arbitrarily combined with any of the illustrated upper limits. In the following description, with respect to certain items Z, the expression "including Z" may include "a form including Z and other items", "a form substantially composed of Z", and "a form composed of Z".
[0017] (Electrochemical Device)
[0018] Hereinafter, the electrochemical device of the present embodiment may be referred to as an “electrochemical device (D)”. The electrochemical device (D) can be used as a power storage device.
[0019] The electrochemical device (D) comprises a positive electrode, a negative electrode and a lithium ion conductive electrolyte. The positive electrode comprises a positive electrode mixture layer containing a positive electrode active material. The positive electrode active material comprises particles of a conductive polymer that can be reversibly doped and dedoped with anions. The particles are sometimes referred to as "particles (P)" hereinafter. When the pore distribution of the positive electrode is measured using a mercury porosimeter, the ratio V1 / V0 of the volume V1 of pores with a pore diameter of less than 0.2 μm to the volume V0 of all pores is greater than 0.40. By setting the ratio V1 / V0 to greater than 0.40, as described in the embodiments, an electrochemical device with high low temperature characteristics can be obtained.
[0020] The volume V1 is the total volume of all pores having a pore diameter of 0.2 μm or less. The volume V0 is the total volume of all pores.
[0021] In the case of an electrochemical device (D), anions are doped into the positive electrode active material (conductive polymer) during charging, and anions are dedoped from the positive electrode active material during discharge. Examples of doping anions into active materials include at least adsorption of anions into active materials. Examples of doping anions into active materials may also include occlusion of anions by active materials, chemical interactions between active materials and anions, and the like.
[0022] When anions are adsorbed on the active material, a double electric layer is formed, showing capacitance. The positive electrode can also be a polarizable electrode. The positive electrode can also be an electrode that has the properties of a polarizable electrode and at the same time, the Faraday reaction also contributes to the positive electrode capacitance.
[0023] As for the negative electrode, for example, cations such as lithium ions can be doped during charging of the electrochemical device, and cations such as lithium ions can be dedoped from the negative electrode during discharging of the electrochemical device. Examples of doping of lithium ions into the negative electrode active material include at least the absorption phenomenon of lithium ions into the negative electrode active material. Examples of doping of lithium ions into the negative electrode active material may also include the adsorption of lithium ions into the negative electrode active material, the chemical interaction between the negative electrode active material and lithium ions, etc.
[0024] If the Faradaic reaction of absorbing lithium ions in the negative electrode active material proceeds, capacitance is exhibited. That is, the electrochemical device (D) has intermediate performance between a lithium ion secondary battery and an electric double layer capacitor, and is similar to a lithium ion capacitor.
[0025] Generally speaking, for electrochemical devices using conductive polymers as active materials, there is a tendency for low-temperature characteristics and drift characteristics to be easily reduced. It is speculated that the low-temperature characteristics and drift characteristics of electrochemical devices are reduced because, during charging, the electrolyte near the active material is easily exhausted, and the internal resistance of the electrode increases. Since conductive polymers are highly hydrophobic, they have low affinity with the electrolyte, and the electrolyte near the active material is easily exhausted. If the internal resistance of the electrode increases, the voltage of the electrochemical device decreases and the capacitance decreases. At low temperatures, the internal resistance tends to be significantly reduced.
[0026] In contrast, for the electrochemical device (D), by setting the ratio V1 / V0 to 0.40 or more, the low temperature characteristics and drift characteristics can be improved. Although the reason is not clear at present, it can be considered that if the proportion of small pores is high, the conductive path is easy to connect and the resistance becomes low. Therefore, it can be considered that by setting the ratio V1 / V0 to 0.40 or more, the low temperature characteristics and drift characteristics can be improved.
[0027] The ratio V1 / V0 may be 0.43 or more, or 0.55 or more. The ratio V1 / V0 may be 1.0 or less, or 0.80 or less, or 0.68 or less. By setting the ratio V1 / V0 to 0.43 or more, the low temperature characteristics of the electrochemical device (D) can be particularly improved.
[0028] The conductive polymer may include a polymer of an aniline compound (aniline), or may be a polymer of an aniline compound. From the perspective of easy doping and dedoping of anions, a polymer of an aniline compound is preferred. However, the conductive polymer may include a conductive polymer other than a polymer of an aniline compound, or may be a conductive polymer other than a polymer of an aniline compound.
[0029] Examples of aniline compounds include aniline (C6H5-NH2) and aniline derivatives. That is, at least one compound selected from aniline and aniline derivatives can be used as the aniline compound. Examples of aniline derivatives include aniline with functional groups (alkyl groups, halogen groups, etc.). The functional group can be at least one selected from alkyl groups and halogen groups. Examples of polymers of aniline compounds include polyaniline and polyaniline derivatives. Examples of polyaniline derivatives include derivatives with alkyl groups such as methyl groups attached to a part of the benzene ring of the aniline unit, derivatives with halogen groups attached to a part of the benzene ring of the aniline unit, etc. In the following, polymers of aniline compounds are sometimes referred to as "polyaniline polymers".
[0030] Polyaniline is a polymer of aniline. Polyaniline is a polymer having an amine structural unit of C6H4-NH-C6H4-NH- and / or an imine structural unit of C6H4-N=C6H4=N-.
[0031] The electrochemical device (D) may further include a current collector (positive electrode current collector) and a carbon layer disposed between the current collector and the positive electrode mixture layer. Specific examples of the carbon layer will be described later. If particles (P) with a smaller average particle size are used in order to make the ratio V1 / V0 greater than 0.40, the adhesion between the current collector and the positive electrode mixture layer is likely to decrease. If their adhesion decreases, manufacturing becomes difficult or the characteristics are reduced. By configuring a carbon layer between the current collector and the positive electrode mixture layer, the adhesion between the current collector and the positive electrode mixture layer can be improved, and the resistance between them can be reduced. When the average particle size of the particles (P) is less than 5 μm, it is particularly preferred to configure a carbon layer between the current collector and the positive electrode mixture layer.
[0032] The carbon layer may contain carboxymethylcellulose ammonium (hereinafter sometimes referred to as "CMC-NH4"). As described later, by using CMC-NH4, the adhesion between the current collector and the positive electrode mixture layer can be improved.
[0033] In the log differential pore volume distribution (logarithmic differential pore volume distribution) of the positive electrode, the maximum peak preferably exists in the region where the pore diameter is less than 0.2 μm. According to this configuration, an electrochemical device with high low temperature characteristics can be obtained. It should be noted that the log differential pore volume distribution is a graph with the horizontal axis being the pore diameter (μm) and the vertical axis being the log differential pore volume (mL / g).
[0034] The average particle size of the particles (P) can be 1 μm or more, or 3 μm or more, and can be 7 μm or less, or 6 μm or less. The average particle size of the particles (P) can be in the range of 3 μm to 6 μm. By setting the average particle size to 7 μm or less (for example, 6 μm or less), it is easy to make the ratio V1 / V0 greater than 0.40. In addition, by setting the average particle size to 3 μm or more, the adhesion between the collector and the positive electrode mixture layer can be improved. Particles (P) having an average particle size of a specified value can be produced by a known method, or commercially available particles can be used.
[0035] The average particle size of the particles (P) is the median diameter (D50) at which the cumulative volume reaches 50% in the volume-based particle size distribution. The median diameter is determined using a laser diffraction / scattering particle size distribution measuring apparatus.
[0036] The negative electrode may include a negative electrode active material that can reversibly store and release lithium ions. Examples of the negative electrode will be described later.
[0037] Examples of the structure and components of the electrochemical device (D) are described below, but the structure and components of the electrochemical device (D) are not limited to the following examples. The electrochemical device (D) may include a positive electrode, a negative electrode, an electrolyte, a separator, and an outer package.
[0038] The electrochemical device (D) may include an electrode group consisting of a positive electrode, a negative electrode, and a separator disposed between the positive electrode and the negative electrode. The electrode group may be a wound type or a stacked type. The wound type electrode group is formed by winding the positive electrode, the negative electrode, and the separator in a manner that the separator is disposed between the positive electrode and the negative electrode. The stacked type electrode group is formed by stacking the positive electrode, the negative electrode, and the separator in a manner that the separator is disposed between the positive electrode and the negative electrode.
[0039] (positive electrode)
[0040] The positive electrode includes a positive electrode mixture layer. The positive electrode may also include a positive electrode current collector and a positive electrode mixture layer. The positive electrode may further include other layers such as a carbon layer.
[0041] (Positive electrode collector)
[0042] The positive electrode current collector may be a sheet-shaped metal material. Examples of sheet-shaped metal materials include metal foil, porous metal, etched metal, etc. Examples of metal materials include aluminum, aluminum alloy, nickel, titanium, etc. The thickness of the positive electrode current collector may be in the range of 10 μm to 100 μm.
[0043] (Carbon layer)
[0044] The carbon layer contains a conductive carbon material. Examples of the conductive carbon material include graphite, hard carbon, soft carbon, carbon black, etc. Carbon black is preferred from the viewpoint of being able to form a thin carbon layer with excellent conductivity. The thickness of the carbon layer may be in the range of 1 μm to 20 μm.
[0045] (Positive electrode mixture layer)
[0046] The positive electrode mixture layer contains conductive polymer particles (P) that can be reversibly doped and dedoped with anions as a positive electrode active material. The conductive polymer is preferably a π-conjugated polymer. As described above, a preferred example of the conductive polymer is a polymer of an aniline compound.
[0047] Examples of π-conjugated conductive polymers other than polymers of aniline compounds include polypyrrole compounds, polythiophene compounds, polyfuran compounds, polythiopheneacetylene compounds, polypyridine compounds, and the like. These "compounds" include not only polyaniline, polypyrrole, polythiophene, polyfuran, polythiopheneacetylene, and polypyridine, but also their derivatives. The so-called derivatives are polymers with polyaniline, polypyrrole, polythiophene, polyfuran, polythiopheneacetylene, and polypyridine as basic skeletons. Derivatives include, for example, derivatives with alkyl groups such as methyl groups attached to a portion of the aromatic ring of each unit, derivatives with halogen groups attached to a portion of the aromatic ring of each unit, and the like. For example, polythiophene derivatives include poly(3,4-ethylenedioxythiophene) (PEDOT), and the like.
[0048] The positive electrode active material only needs to contain at least one of the above-mentioned conductive polymers, but preferably contains a polyaniline polymer (polyaniline). The content of the polyaniline polymer in the conductive polymer contained in the positive electrode active material is preferably 50% by mass or more. The content may also be 80% by mass or more, 90% by mass or more. The content is 100% by mass or less, or 100% by mass. All the conductive polymers contained in the positive electrode active material may be polyaniline polymers.
[0049] The weight average molecular weight of the conductive polymer (eg, polyaniline-based polymer) is not particularly limited, and may be in the range of 1,000 to 100,000.
[0050] Conductive polymers may contain dopants. By doping the π-electron conjugated polymer with a dopant, excellent conductivity is exhibited. Examples of anions (dopants) that can be doped and dedoped in the conductive polymer include nitrate ions, phosphate ions, borate ions, benzenesulfonate ions, naphthalenesulfonate ions, toluenesulfonate ions, and methanesulfonate ions (CF3SO3 - ), perchlorate ion (ClO4 - ), tetrafluoroborate ion (BF4 - ), hexafluorophosphate ion (PF6 - ), fluorosulfate ion (FSO3 - ), bis(fluorosulfonyl)imide ion (N(FSO2)2 - ), bis(trifluoromethanesulfonyl)imide ion (N(CF3SO2)2 - ) etc. These anions may be used alone or in combination of two or more.
[0051] From the perspective of easy reversible doping and dedoping in conductive polymers, PF6 is preferably used. - As anions. More than 90 mol% of all anions contained in the electrolyte can be PF6 - As the iminium ion, N(FSO2)2 is preferred. - .
[0052] The anion (dopant) may also be a polymer ion. Examples of the polymer ion include anions of polyvinyl sulfonic acid, polystyrene sulfonic acid, polyallyl sulfonic acid, polyacryloyl sulfonic acid, polymethacryloyl sulfonic acid, poly(2-acrylamide-2-methylpropane sulfonic acid), polyisoprene sulfonic acid, polyacrylic acid, etc. These may be homopolymers or copolymers of two or more monomers. These may be used alone or in combination of two or more.
[0053] The particles (P) of the conductive polymer can use commercially available particles. Alternatively, the conductive polymer can also be synthesized by electrolytic polymerization or chemical polymerization in a reaction solution containing raw material monomers of the conductive polymer. For example, by adding an oxidant to the reaction solution containing the raw material monomers, the conductive polymer can be chemically polymerized. The raw material monomers of the conductive polymer can be selected according to the conductive polymer to be synthesized. Examples of monomers include aniline, pyrrole, thiophene, furan, thiophene acetylene, pyridine and their derivatives. The raw material monomers may also include oligomers.
[0054] Electrolytic polymerization or chemical polymerization can be carried out using a reaction solution containing a dopant. Thus, the amount of anions doped in the conductive polymer during charging of the electrochemical device can be increased. However, the dopant (e.g., sulfate ion) used during electrolytic polymerization or chemical polymerization does not need to be the same as the dopant constituting the electrochemical device (D). For example, after electrolytic polymerization is carried out in a reaction solution containing sulfate ions and raw material monomers, sulfate ions can be dedoped. Thus, the amount of anions doped in the conductive polymer during charging of the electrochemical device can be increased.
[0055] The positive electrode mixture layer (or the electrolyte) may contain sulfate ions (SO4 2- ). Even in this case, by including a nonionic surfactant in the electrolyte, the decrease in drift characteristics can be suppressed.
[0056] The positive electrode mixture layer may contain additives. Examples of additives include binders, conductive materials, and thickeners. Conductive materials include, for example, granular carbon materials such as carbon black, carbon fibers, carbon nanotubes, fibrous carbon materials such as carbon nanofibers, etc. Examples of carbon black include acetylene black, Ketjen black, furnace black, etc. Among them, acetylene black and Ketjen black are preferred. Considering the small amount of impurities, acetylene black is more preferred.
[0057] Examples of binders include polycarboxylic acids, carboxymethyl cellulose, derivatives of carboxymethyl cellulose, fluororesins, rubber materials, etc. Examples of derivatives of carboxymethyl cellulose include sodium carboxymethyl cellulose, ammonium carboxymethyl cellulose, etc. As polycarboxylic acids, acrylic resins such as polyacrylic acid, polymethacrylic acid, and acrylic acid-methacrylic acid copolymers, and alginic acid can be cited. As fluororesins, polyvinylidene fluoride, polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymers, etc. can be cited. As rubber materials, styrene-butadiene rubber (SBR) can be cited. These binders can be used alone or in combination.
[0058] The content of the conductive polymer in the positive electrode mixture layer may be in the range of 60 to 90% by mass. The content of the conductive material in the positive electrode mixture layer may also be in the range of 1 to 30% by mass. The content of the binder in the positive electrode mixture layer may be in the range of 1 to 10% by mass.
[0059] (negative electrode)
[0060] The negative electrode includes a negative electrode mixture layer. The negative electrode may include a negative electrode current collector and a negative electrode mixture layer disposed on the negative electrode current collector.
[0061] (Negative electrode current collector)
[0062] The negative electrode current collector uses a sheet-like metal material. Examples of sheet-like metal materials include metal foil, porous metal, and etched metal. Examples of metal materials include copper, copper alloys, nickel, and stainless steel. The thickness of the negative electrode current collector can be in the range of 10 μm to 100 μm.
[0063] (Negative electrode mixture layer)
[0064] The negative electrode mixture layer contains a negative electrode active material and may further contain other additives (a binder, a conductive material, a thickener, etc.). The conductive material and the binder may be those exemplified in the description of the positive electrode mixture layer.
[0065] Examples of negative electrode active materials include materials that electrochemically absorb and release lithium ions. Examples of such materials include carbonaceous materials, metal compounds, alloys, ceramic materials, etc. Among them, carbonaceous materials are preferred from the perspective of being able to reduce the potential of the negative electrode. As carbonaceous materials, graphite, hard carbon, and soft carbon are preferred, and hard carbon is particularly preferred. The d value of the (002) plane of hard carbon obtained from the X-ray diffraction pattern is greater than 0.38nm. Hard carbon is preferred from the perspective of having lower resistance and higher capacitance than graphite.
[0066] There is no limitation on the method for forming the negative electrode mixture layer, and it can be formed by a known method. For example, the negative electrode mixture layer can be formed by the following method. First, the constituent components of the negative electrode mixture layer are mixed with a dispersion medium to prepare a negative electrode mixture slurry. Then, the negative electrode mixture slurry is applied to the negative electrode collector to form a coating film. Then, the negative electrode mixture layer can be formed by drying the coating film. The coating film can be rolled as needed. The dispersion medium is not particularly limited, and water or a non-aqueous solvent can be used, or a mixture thereof can be used. The thickness of the negative electrode mixture layer is not particularly limited, and it can be in the range of 10μm to 300μm.
[0067] The negative electrode mixture layer is preferably pre-doped with lithium ions. This lowers the potential of the negative electrode, thereby increasing the difference between the potential of the positive electrode and the potential of the negative electrode (ie, the voltage), and improving the energy density of the electrochemical device.
[0068] The pre-doping of lithium ions into the negative electrode can be performed using the following method. First, a metal lithium layer that serves as a lithium ion supply source is formed on the surface of the negative electrode mixture layer. Then, the negative electrode having the metal lithium layer is immersed in an electrolyte having lithium ion conductivity. At this time, lithium ions are dissolved from the metal lithium layer into the non-aqueous electrolyte, and the dissolved lithium ions are absorbed by the negative electrode active material. For example, when graphite or hard carbon is used as the negative electrode active material, lithium ions are inserted into the interlayers of graphite and the pores of hard carbon. By performing such operations, lithium ions are pre-doped. The amount of pre-doped lithium ions can be controlled by the mass of the metal lithium layer. The amount of pre-doped lithium can be in the range of 50% to 95% of the maximum amount that can be absorbed by the negative electrode mixture layer.
[0069] The process of pre-doping the negative electrode with lithium ions may be performed before assembling the electrode group, or may be performed after the electrolyte solution and the electrode group are housed in an outer package.
[0070] (Diaphragm)
[0071] The separator is not particularly limited, and a separator used in a known power storage device can be used. Examples of separators include nonwoven fabrics made of cellulose fibers, nonwoven fabrics made of glass fibers, microporous films made of polyolefins, woven fabrics, and nonwoven fabrics. The thickness of the separator can be in the range of 10 μm to 300 μm (e.g., in the range of 10 μm to 40 μm).
[0072] (Electrolytes)
[0073] The electrolyte has lithium ion conductivity. The electrolyte contains a non-aqueous solvent, a lithium salt, and a non-ionic surfactant. The lithium salt is a salt of lithium ions and anions, and the anions from the lithium salt are doped into the positive electrode when the electrochemical device is charged.
[0074] Examples of lithium salts include lithium bis(fluorosulfonyl)imide (LiN(SO2F)2) (hereinafter sometimes referred to as "LIFSI"), LiClO4, LiBF4, LiPF6, LiAlCl4, LiSbF6, LiSCN, LiCF3SO3, LiFSO3, LiCF3CO2, LiAsF6, LiB 10 Cl 10 , LiCl, LiBr, LiI, LiBCl4, LiN(CF3SO2)2, etc. These may be used alone or in combination of two or more.
[0075] The lithium salt may include at least one selected from LIFSI, LiPF6 and LiBF4. These lithium salts are preferred from the perspective of high stability and no effect on nonionic surfactants. In addition, these lithium salts are also preferred from the perspective of high dissociation degree and excellent ion conductivity. Among them, LIFSI is more preferred from the perspective of particularly high stability.
[0076] The nonaqueous solvent is not particularly limited and can be appropriately selected according to purpose. For example, as the non-aqueous solvent, cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate, chain carbonates such as dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), aliphatic carboxylates such as methyl formate, methyl acetate, methyl propionate (PC), and ethyl propionate, lactones such as γ-butyrolactone and γ-valerolactone, chain ethers such as 1,2-dimethoxyethane (DME), 1,2-diethoxyethane (DEE), and ethoxymethoxyethane (EME), cyclic ethers such as tetrahydrofuran and 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, acetamide, dimethylformamide, dioxolane, acetonitrile, propionitrile, nitromethane, ethyl monoglyme, trimethoxymethane, sulfolane, methyl sulfolane, 1,3-propane sultone, and the like can be used. These may be used alone or in combination of two or more.
[0077] The electrolyte may contain additives as necessary. For example, unsaturated carbonates such as vinylene carbonate, vinylethylene carbonate, and divinylethylene carbonate may be used as additives for forming a film having high lithium ion conductivity on the surface of the negative electrode.
[0078] (Outer packaging)
[0079] The outer casing is not particularly limited, and any outer casing used in a known power storage device can be used. The outer casing can be composed of a metal case, a gasket, a sealing body, and the like.
[0080] (Manufacturing method of positive electrode)
[0081] An example of a method for manufacturing a positive electrode is described below. Hereinafter, the manufacturing method is sometimes referred to as "manufacturing method (M)". According to the manufacturing method (M), the positive electrode of the electrochemical device (D) can be manufactured. However, the positive electrode of the electrochemical device (D) can also be manufactured using a method other than the manufacturing method (M). Since the matters described for the positive electrode of the electrochemical device (D) can be applied to the manufacturing method (M), repeated descriptions are sometimes omitted. In addition, the matters described for the manufacturing method (M) can also be applied to the positive electrode of the electrochemical device (D).
[0082] The manufacturing method (M) includes steps (i) and (ii). Step (i) is a step of preparing a positive electrode mixture slurry by mixing the constituents of the positive electrode mixture layer with a dispersion medium. The constituents of the positive electrode mixture layer include particles (P) of a conductive polymer that can be reversibly doped and dedoped with anions. The constituents of the positive electrode mixture layer include other additives (binders, conductive materials, thickeners, etc.) as needed. The dispersion medium can use water, an organic solvent (e.g., N-methyl-2-pyrrolidone (NMP)), or a mixture thereof.
[0083] The particles (P) can use particles (P) having the above-mentioned average particle size. By selecting the average particle size of the particles (P) used in step (i), the average particle size (P) of the particles (P) in the positive electrode mixture layer can be controlled. In addition, by changing the ratio of the components in the positive electrode mixture slurry, the content of each component in the positive electrode mixture layer can be controlled. Thus, the ratio of each component in the positive electrode mixture layer can be selected according to the content of each component in the formed positive electrode mixture layer.
[0084] Step (ii) is a step of forming a positive electrode mixture layer on a positive electrode current collector using a positive electrode mixture slurry. The method for forming the positive electrode mixture layer is not particularly limited, and a known method can be used. In one example method, first, the positive electrode mixture slurry is applied to the positive electrode current collector to form a coating. Then, the positive electrode mixture layer can be formed by drying the coating. The slurry coating method is not particularly limited, and a known coating method can be used. The drying step is not particularly limited, as long as the drying conditions are selected according to the dispersion medium. For example, the coating can be dried by heating it at 90°C for 5 minutes. In addition, it can also be dried under reduced pressure.
[0085] Step (ii) may include a step of pressing the coating film after drying. The pressing pressure may be 200 kgf / cm 2 ~600kgf / cm 2 range (range of 19.6MPa~58.8MPa).
[0086] In the manufacturing method (M), the positive electrode mixture layer is formed in such a manner that the ratio V1 / V0 is the above-mentioned value (0.40 or more). By pressing the coating film that becomes the positive electrode mixture layer, the value of the ratio V1 / V0 can be increased. The pressing pressure can be selected according to the target value of the ratio V1 / V0. In addition, by using particles (P) with a small average particle size, the value of the ratio V1 / V0 can be increased. The average particle size of the particles (P) used in the manufacturing method (M) can be within the above-mentioned range.
[0087] A conductive layer such as a carbon layer can be formed on the positive electrode collector. In this case, a positive electrode mixture layer is formed on the positive electrode collector via a conductive layer. The carbon layer can be formed using the following method. First, particles of a conductive carbon material are mixed with a dispersion medium to prepare a carbon slurry. Additives (thickeners, etc.) can be added to the carbon slurry. As a thickener, ammonium carboxymethyl cellulose (CMC-NH4) is preferred. The dispersion medium can use water or a liquid containing water.
[0088] Then, after the carbon slurry is applied to the positive electrode collector to form a coating, the coating is dried to form a carbon layer. The coating method of the slurry is not particularly limited, and a known coating method can be used. Drying is preferably performed at a temperature of 130° C. or higher (e.g., in the range of 130 to 170° C.). By drying (heat treatment) at this temperature, at least a portion of the CMC-NH4 can be separated from ammonia and converted into carboxymethyl cellulose (hereinafter sometimes referred to as "CMC").
[0089] CMC has lower solubility in water than CMC-NH4. Therefore, by converting CMC-NH4 into CMC during the drying process, the adhesion between the carbon layer and the positive electrode current collector can be improved. In addition, even if an aqueous positive electrode mixture slurry is applied when forming a positive electrode mixture layer on the carbon layer, since the carbon layer is not easily soluble in water, the adhesion between the carbon layer and the positive electrode mixture layer can be improved.
[0090] On the other hand, with regard to the addition of CMC to a carbon slurry containing water as a dispersion medium, there is a problem of low solubility of CMC in water. Sodium carboxymethylcellulose (hereinafter sometimes referred to as "CMC-Na") has a high solubility in water compared to CMC. However, CMC-Na is different from CMC-NH4 and basically does not become CMC due to heating during drying. Therefore, from the perspective of improving the adhesion between the carbon layer and the positive electrode collector, it is more preferable to use CMC-NH4 than to use CMC-Na.
[0091] The positive electrode and other components manufactured as described above can be used to manufacture an electrochemical device (D). For example, first, an electrode group is formed using a positive electrode, a negative electrode, and a separator. Then, the electrode group and an electrolyte (electrolyte) are sealed in an outer packaging body. By operating in this way, an electrochemical device (D) can be manufactured.
[0092] Hereinafter, an example of an electrochemical device (D) is specifically described with reference to the accompanying drawings. The above-mentioned components can be applied to the components of the electrochemical device (D) of the example described below. In addition, in the example described below, components that are not essential in the electrochemical device (D) can be omitted.
[0093] Figure 1 1 is a schematic diagram showing a cross section of the electrochemical device 100 according to the present embodiment. Figure 2 It is a schematic diagram showing a partial development of the electrode group 10 included in the electrochemical device 100 .
[0094] like Figure 1 As shown, the electrochemical device 100 includes an electrode group 10, a container 101, a sealing body 102, a seat plate 103, leads 104A and 104B, and lead connectors 105A and 105B. The container 101 accommodates the electrode group 10. The sealing body 102 blocks the opening of the container 101. The seat plate 103 covers the sealing body 102. The lead connectors 105A and 105B respectively connect the leads 104A and 104B to each electrode of the electrode group 10. The vicinity of the open end of the container 101 is drawn inward. The open end is curled in a manner riveted to the sealing body 102.
[0095] The electrode group 10 includes a positive electrode 11, a negative electrode 12, and a separator 13 disposed therebetween. The positive electrode 11 and the negative electrode 12 are wound with the separator 13 disposed therebetween to form a wound body. The outermost periphery of the wound body is fixed with a stop tape 14. It should be noted that Figure 2 The partially unfolded state is shown before the outermost circumference of the wound body is fixed.
[0096] Example
[0097] Hereinafter, the electrochemical device of the present disclosure will be described in further detail using examples. In this example, a plurality of electrochemical devices (devices A1 to A7 and C1 to C2) were produced and evaluated.
[0098] (Device A1)
[0099] Device A1 was manufactured by the following method.
[0100] (1) Preparation of positive electrode
[0101] First, carbon black, carboxymethyl cellulose ammonium (CMC-NH4) and water are mixed at a ratio of carbon black: CMC-NH4: water = 6:3:90 (mass ratio) to prepare a carbon slurry. Then, the carbon slurry is applied on both sides of an aluminum foil (thickness: 30 μm) to form a coating. Then, the coating is heated at 170°C for 2 hours to form a carbon layer. By operating in this way, a positive electrode core material comprising a positive electrode collector and a carbon layer is obtained.
[0102] The positive electrode mixture slurry is prepared by mixing a dispersion of a conductive polymer (positive electrode active material), carbon black (conductive material), a dispersion of styrene-butadiene rubber (binder), and a solution of carboxymethyl cellulose (thickener). The mixing ratio of the conductive polymer, carbon black, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC) in the positive electrode mixture slurry is set to conductive polymer: carbon black: SBR: CMC = 75:15:7:3 (mass ratio).
[0103] The conductive polymer particles (particles (P)) used polyaniline particles with an average particle size (D50) of 3 μm. The carbon black dispersion liquid consisted of carbon black and water, with a mass ratio of carbon black: water = 20:80. Acetylene black was used for carbon black. The SBR dispersion liquid consisted of SBR and water, with SBR: water = 40:60 (mass ratio). The CMC solution consisted of CMC and water, with CMC: water = 3:97 (mass ratio).
[0104] Then, the positive electrode mixture slurry is applied to both sides of the positive electrode core material to form a coating. Then, the coating is heated at a temperature of about 60 to 90°C. After heating, the coating is pressed using a roller press and then vacuum dried at 110°C for 12 hours. Pressing is performed at 500kgf / cm 2 By doing so, a positive electrode mixture layer (thickness: 30 μm) was formed on both sides of the core material. By doing so, a positive electrode having a positive electrode mixture layer formed on a positive electrode current collector via a carbon layer was obtained.
[0105] (2) Preparation of negative electrode
[0106] 97 parts by mass of hard carbon, 1 part by mass of carboxycellulose and 2 parts by mass of styrene-butadiene rubber were mixed, and the resulting mixed powder and water were kneaded to prepare negative electrode mixture slurry. The mixed powder and water were mixed at a mixed powder:water=40:60 (mass ratio).
[0107] Then, the negative electrode mixture slurry is applied to both sides of the negative electrode collector to form a coating. A copper foil with a thickness of 20 μm is used as the negative electrode collector. Then, the coating is dried to form a negative electrode mixture layer. By operating in this way, a strip-shaped negative electrode having a negative electrode mixture layer (thickness: 35 μm) on both sides is obtained. Then, a metallic lithium layer is formed on the negative electrode mixture layer. The amount of the metallic lithium layer is set to an amount calculated so that the negative electrode potential in the electrolyte after pre-doping is completed is less than 0.2 V relative to metallic lithium.
[0108] (3) Preparation of electrode group
[0109] Lead tabs were connected to the positive electrode and the negative electrode, respectively. Then, the positive electrode, the negative electrode, and the separator were wound to produce an electrode group (wound body). The separator was arranged between the positive electrode and the negative electrode. A nonwoven fabric made of cellulose fiber (thickness 35 μm) was used as the separator.
[0110] (4) Preparation of electrolyte
[0111] In a dry argon atmosphere, propylene carbonate and dimethyl carbonate were mixed at a volume ratio of 1:1 to obtain a mixture. 0.2% by mass of vinylene carbonate was added to the mixture to prepare a solvent. LiPF6 was dissolved as a lithium salt in the obtained solvent. By performing the operation in this way, a solvent having hexafluorophosphate ions (PF6 - ) electrolyte. The concentration of LiPF6 in the electrolyte was set to 1.5 mol / L.
[0112] (5) Fabrication of electrochemical device
[0113] The electrode group and the electrolyte were placed in an open bottomed container to assemble an electrochemical device. Thereafter, a charging voltage of 3.8 V was applied between the positive electrode terminal and the negative electrode terminal, and the device was aged at 25° C. for 24 hours. The negative electrode was pre-doped with lithium ions by the aging. By performing the operation in this way, a device A1 was produced.
[0114] (Evaluation of characteristics)
[0115] The characteristics of the device A1 were evaluated by the following method.
[0116] (1) Determination of pore size distribution
[0117] The pore distribution of the positive electrode formed to make device A1 is measured using the following steps. First, the device A1 is discharged until its voltage reaches the lower limit of the rated voltage. At this time, the dopant is dedoped from the conductive polymer. Thereafter, the device A1 is disassembled and the positive electrode is taken out, which is then washed with a low-boiling point solvent such as dimethyl carbonate (DMC) and dried. Then, a portion (width and length are approximately 1.25 and 2.5 cm, respectively) is cut out from the positive electrode to obtain a sample. About 0.6 g of the sample is placed in a large sample cell with a volume of 5 cc (the main volume is 0.4 cc).
[0118] Then, the pore distribution (pore volume distribution) of the sample in the sample cell was measured using a mercury porosimeter. Auto Pore IV manufactured by Shimadzu Corporation was used in the measurement. The measurement was carried out under the condition of an initial pressure of 4 kPa. As shown above, the pore distribution of the sample having a positive electrode mixture layer formed on both sides of the positive electrode core material was measured. In this case, it is considered that the influence of the positive electrode core material on the measurement results of the pore distribution can be ignored.
[0119] Based on the above measurement results, the volume V1, volume V2 and ratio V1 / V0 were calculated. Volume V2 is the volume of pores with a pore diameter greater than 0.2 μm. Volume V0 is equal to the sum of volume V1 and volume V2. In addition, based on the above measurement results, it was confirmed whether the maximum peak in the log differential pore volume distribution exists in the region with a pore diameter of less than 0.2 μm.
[0120] (2) Initial internal resistance (DCR)
[0121] In an environment of -30°C, device A1 was charged to 3.6V and then discharged to 2.5V. The initial internal resistance R1 at -30°C was determined using the voltage drop and discharge current during the predetermined discharge time.
[0122] (3) DCR retention rate
[0123] Device A1 is charged at a voltage of 3.6V at 25°C. Thereafter, device A1 is charged to 3.6V at 60°C and placed in this environment for 1000 hours. Thereafter, device A1 is placed in a -30°C environment, and the voltage drop and discharge current are measured when the discharge is performed for a specified time. Thereafter, the voltage drop and the discharge current are used to calculate the internal resistance R2 at -30°C after the high temperature placement test. Using the initial internal resistance R1 and the internal resistance R2, the DCR retention rate is calculated by the following formula. The closer the DCR retention rate is to 100, the smaller the change in internal resistance and the better the drift characteristics.
[0124] DCR retention rate (%) = 100 × R2 / R1
[0125] (4) Initial capacitance
[0126] After charging the device A1 at 3.6 V in an environment of -30°C, the device A1 was discharged until the voltage of the device A1 reached 2.5 V. In this process, the amount of discharge charge flowing during the period when the voltage of the device A1 dropped from 3.3 V to 3.0 V was divided by the voltage change ΔV (= 0.3 V), thereby obtaining the initial capacitance at low temperature.
[0127] (Device A2~A7 and C1~C2)
[0128] Devices A2 to A7 and C1 to C2 were produced in the same manner as device A1 except that the manufacturing conditions of the positive electrode were changed. Specifically, the positive electrode was produced by changing the value of the ratio V1 / V0, the presence or absence of the formation of the carbon layer, and the presence or absence of the pressing of the coating film that would become the positive electrode mixture layer as shown in Table 1. The ratio V1 / V0 was changed by the average particle size of the particles (P) and / or the presence or absence of the pressing of the coating film that would become the positive electrode mixture layer. The pressing of the coating film was carried out at 500 kgf / cm 2 However, in the production of the positive electrodes of the devices A3 and A7, the coating film that would become the positive electrode mixture layer was not pressed.
[0129] It should be noted that an attempt was made to produce a positive electrode under the same conditions as the positive electrode of device A1 except that a carbon layer was not formed on the surface of the positive electrode collector. However, in this case, the coating of the positive electrode mixture peeled off from the positive electrode collector, and a usable positive electrode could not be obtained. On the other hand, in the production of the positive electrodes of devices A1 to A7 and C1 to C2, no peeling of the coating from the positive electrode collector occurred.
[0130] The manufactured devices A2 to A7 and C1 to C2 were also evaluated in the same manner as the device A1. However, the DCR retention rate of the devices C1 and C2 was not evaluated.
[0131] Part of the manufacturing conditions of each device and part of the evaluation results are shown in Table 1. It should be noted that the so-called "presence or absence of a peak" in Table 1 indicates whether the maximum peak exists in the region with a pore diameter of 0.2 μm or less in the log differential pore volume distribution curve. If the maximum peak exists in the region with a pore diameter of 0.2 μm or less, it is set as "presence", and if it does not exist, it is set as "no". In Table 1, "pressing of the coating film" means pressing of the coating film that becomes the positive electrode mixture layer.
[0132] Table 1
[0133]
[0134] The evaluation results of the characteristics of the device are shown in Table 2. The values of the initial internal resistance R1 and the initial capacitance are relative values when the value of the device C1 is set to 100.0.
[0135] Table 2
[0136]
[0137] As shown in Table 2, devices A1 to A7 having a ratio V1 / V0 of 0.40 or more have significantly improved characteristics compared to devices C1 and C2 of the comparative example having a ratio V1 / V0 of less than 0.40. Specifically, devices A1 to A7 have low initial internal resistance at low temperatures and high initial capacitance at low temperatures.
[0138] When the ratio V1 / V0 is in the range of 0.53 to 0.68, the initial internal resistance R1 becomes particularly low. When the ratio V1 / V0 is 0.65 or more, the initial capacitance becomes particularly high.
[0139] For the device A4 without a carbon layer, the DCR retention rate was much higher than 100, and the characteristics were greatly reduced. On the other hand, for the devices A1 to A3 with a carbon layer, the increase in the DCR retention rate was small. For the device using CMC-NH4 as a thickener for the carbon layer, the DCR retention rate was significantly higher than that of the device using CMC-NH4. a As compared with the device used as a thickener for the carbon layer, the increase in the DCR retention rate can be suppressed.
[0140] Comparison between the case where the coating was pressed and the case where the coating was not pressed shows that the ratio V1 / V0 can be improved by pressing the coating. In addition, the ratio V1 / V0 can be improved by using particles (P) with a small average particle size.
[0141] Industrial Applicability
[0142] The present disclosure may be used in electrochemical devices.
[0143] Although the present invention has been described with respect to the present preferred embodiments, the above disclosure should not be interpreted in a limiting sense. Upon reading the above disclosure, various modifications and changes will undoubtedly be apparent to those skilled in the art to which the technical field of the present invention belongs. Therefore, the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.
[0144] Description of Reference Numerals
[0145] 10 electrode group, 11 positive electrode, 12 negative electrode, 13 separator, 22 negative electrode, 100 electrochemical device.
Claims
1. An electrochemical device comprising a positive electrode, a negative electrode and a lithium ion conductive electrolyte, The positive electrode comprises a positive electrode mixture layer containing a positive electrode active material. The positive electrode active material includes conductive polymer particles that can be reversibly doped and dedoped with anions. When the pore distribution of the positive electrode is measured by a mercury porosimeter, a ratio V1 / V0 of the volume V1 of pores having a pore diameter of 0.2 μm or less to the volume V0 of all pores is 0.40 or more.
2. The electrochemical device according to claim 1, wherein: The conductive polymer includes a polymer of an aniline compound. 3 . The electrochemical device according to claim 1 , further comprising a current collector and a carbon layer disposed between the current collector and the positive electrode mixture layer.
4. The electrochemical device according to claim 3, wherein: The carbon layer comprises ammonium carboxymethylcellulose.
5. The electrochemical device according to any one of claims 1 to 4, wherein In the log differential pore volume distribution of the positive electrode, the maximum peak exists in a region where the pore diameter is 0.2 μm or less.
6. The electrochemical device according to any one of claims 1 to 5, wherein The average particle size of the particles is 7 μm or less.
7. The electrochemical device according to any one of claims 1 to 6, wherein The negative electrode includes a negative electrode active material that reversibly stores and releases lithium ions.