Acetylene purification adsorbent as well as preparation method and application thereof
The porous adsorbent prepared by acetylene carbon black and BDO tar solves the problem of purifying higher acetylene in the acetylene tail gas in the acetylene aldehyde process, realizes the utilization of waste resources, and improves the economic value of acetylene recovery.
Patent Information
- Application Number
- CN202410939437.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-10-15
AI Technical Summary
In the existing BDO production process by the acetylenic aldehyde method, the propadiene content in the acetylene tail gas is high, which makes acetylene recovery and purification difficult. The traditional purification method has the problems of high temperature treatment, multi-step operation and large acetylene loss.
Porous materials are prepared by blending acetylene carbon black and BDO tar, and are modified by sodium bicarbonate aqueous solution and then mixed and roasted with basic metal salts to prepare a porous adsorbent with strong high-grade acetylene adsorption capacity, which can be used for the purification of acetylene-rich tail gas.
It achieves the efficient removal of high-grade acetylene in acetylene-rich tail gas, improves the purification effect of acetylene, utilizes waste resources, and improves the economic value of the industrial chain.
Smart Images

Figure BDA0004943564120000081 
Figure BDA0004943564120000082 
Figure BDA0004943564120000091
Abstract
Description
Technical Field
[0001] The present invention relates to an adsorbent and a preparation method and application thereof, and in particular to an acetylene purification adsorbent and a preparation method and application thereof. Background Art
[0002] In the acetylene-formaldehyde process for producing BDO (1,4-butanediol), acetylene and formaldehyde are used as raw materials in the presence of a copper-bismuth catalyst to produce the intermediate product, 1,4-butynediol. To maintain the acetylene concentration, a continuous purge gas must be discharged. This purge gas comprises approximately 50% by volume of acetylene, with the remainder consisting of impurities such as nitrogen, carbon dioxide, and propadiene. Due to the reactive nature of the acetylene in this waste gas, direct disposal is dangerous, difficult, and results in significant economic losses. Recovering and recycling the acetylene is key to resolving this issue, but the propadiene must be removed before the waste gas can be returned to the acetylene plant for reuse. Otherwise, the propadiene will accumulate in the acetylene plant, severely impacting reaction efficiency.
[0003] Currently, there are relatively few propylene removal processes. Due to the high propylene content in the tail gas, there are no actual cases for industrial application. Patent CN115181001A removes impurities from acetylene raw material gas for the first time under cryogenic conditions of -42°C to -28°C and a pressure of 0.1MPa to 0.15MPa to obtain crude acetylene raw material, which is then passed into a primary adsorption tower filled with coal-based activated carbon adsorbent, and subjected to a second impurity removal at a temperature of 15°C to 25°C and a pressure of 0.1MPa to 0.15MPa to obtain a primary acetylene crude product, which is then passed into a secondary adsorption tower filled with silica gel adsorbent, and subjected to a third impurity removal at a temperature of 15°C to 25°C and a pressure of 0.1MPa to 0.15MPa to obtain refined acetylene. After filtering out particulate matter through a filter, the product is passed into a buffer tank, and then pressurized and filled with a compressor to obtain high-purity acetylene. However, this method has large purification temperature variations, many steps, and complicated operations. In addition, the raw material itself contains a large amount of impurities, with a relatively small proportion of propadiene.
[0004] Patent CN108238841A discloses a method of purifying acetylene with sulfuric acid to remove impurities such as propadiene. However, this method involves strong acids and bases, and the loss of acetylene is large. Therefore, it is of practical significance to develop a new acetylene purification solution. Summary of the Invention
[0005] To address the above technical problems, the present invention provides an acetylene purification adsorbent, its preparation method, and its application. Through continuous research, the inventors discovered that a porous material prepared by blending acetylene black and BDO tar, then modifying it with an aqueous sodium bicarbonate solution, and finally mixing it with a basic metal salt and calcining it, can produce a porous adsorbent with strong adsorption capacity for higher acetylenes. This material is excellent for purifying acetylene-rich tail gas containing higher acetylenes.
[0006] Acetylene is typically produced from natural gas through hydrocarbon cracking, a highly endothermic process. The resulting acetylene easily decomposes and polymerizes at high temperatures, producing a large amount of carbon black, composed of 98-99wt% inorganic carbon, 1-2wt% benzene series, and higher hydrocarbons above C10. This carbon black is typically exported to power plants as a carbon source for combustion and power generation, resulting in relatively low added value.
[0007] Furthermore, in the industrial production of BDO, acetylene and formaldehyde react under catalytic conditions to produce 1,4-butynediol, which is then hydrogenated to produce crude BDO, which is then further concentrated and refined to produce the BDO product. However, due to impurities in the synthetic raw materials and byproducts produced during the acetylene-aldehyde reaction and hydrogenation, the refining process of crude BDO produces a large amount of tar, the main components of which are difficult-to-process polymers and inorganic salt ions. If this tar is treated using traditional incineration methods, the inorganic salts melt into droplets at high temperatures and adhere to the outer walls of the heat exchange tubes in the boiler, affecting heat transfer efficiency. Furthermore, the recovered steam quality is unstable, making it difficult to use in production.
[0008] The present invention uses acetylene carbon black and BDO tar to prepare the adsorbent, which has a loose structure, a large specific surface area, and a strong adsorption capacity for higher-order alkynes. It not only solves the technical difficulties of removing higher-order alkynes from acetylene-rich tail gas and purifying acetylene, but also realizes new resource utilization of waste, which is conducive to enhancing the economic value of the device and the industrial chain.
[0009] To achieve the above object, the technical solutions adopted by the present invention are as follows:
[0010] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0011] 1) Weighing and mixing acetylene black and BDO tar, and then heating them under an inert atmosphere to obtain a porous material; the weight ratio of the acetylene black and BDO tar is (0.1-10):1, preferably (0.5-2):1;
[0012] 2) The porous material obtained in step 1) is crushed and then immersed in a sodium bicarbonate aqueous solution for modification. After the treatment, the solid is filtered out, dried, mixed with a basic metal salt, and calcined to obtain the adsorbent.
[0013] As a preferred embodiment of the preparation method of the present invention, in step 1), the heating treatment temperature is 300-1000° C., preferably 500-800° C., and the heating treatment time is preferably 1-24 h, preferably 1-3 h;
[0014] Preferably, the heating treatment is carried out according to a heating-cooling procedure, which is repeated 1-10 times, preferably 1-3 times;
[0015] Preferably, the inert atmosphere is provided by nitrogen and / or argon.
[0016] As a preferred embodiment of the preparation method of the present invention, the acetylene black is a by-product carbon black derived from the natural gas process for producing acetylene, and preferably comprises 98-99 wt% of inorganic carbon, 1-2 wt% of benzene series and higher hydrocarbons above C10;
[0017] Preferably, the BDO tar is a byproduct tar produced by the acetylene aldehyde process for producing 1,4-butanediol, and preferably comprises 1-25 wt% of 1,4-butanediol, 1-5 wt% of an alkali metal salt (such as sodium formate, sodium carbonate, etc.), and 70-98 wt% of a polymer.
[0018] As a preferred embodiment of the preparation method of the present invention, in step 2), the porous material is crushed to 20-500 mesh, preferably 200-400 mesh;
[0019] Preferably, the concentration of the sodium bicarbonate aqueous solution is 1-20 wt%, preferably 5-10 wt%.
[0020] The sodium bicarbonate modification in this invention can reduce the surface acidic sites of the adsorbent and enhance the surface basic sites, thereby improving the adsorption capacity for higher alkynes and preventing acetylene polymerization at the acidic sites. Furthermore, the sodium bicarbonate decomposes during the subsequent calcination process to form a fluffy structure, increasing the specific surface area of the adsorbent.
[0021] As a preferred embodiment of the preparation method of the present invention, the modification method in step 2) is ultrasonic treatment for 1-5 hours. Preferably, the ultrasonic frequency is 80-120 Hz and the treatment time is 1-4 hours.
[0022] As a preferred embodiment of the preparation method of the present invention, in step 2), the amount of the basic metal salt is 0.1-10 wt %, preferably 0.5-2 wt %, of the mass of the porous material before modification;
[0023] Preferably, the basic metal salt is a basic carbonate selected from any one or more of copper, bismuth, and lead, preferably one or more of basic copper carbonate, basic bismuth carbonate, and basic lead carbonate. The mixed modification of the basic metal salts in the present invention can further enhance the adsorption capacity of the adsorbent for higher alkynes.
[0024] As a preferred embodiment of the preparation method of the present invention, the calcination in step 2) is a gradient calcination, preferably a three-stage calcination, the first, second and third stage calcination temperatures are 120-170°C, 220-320°C, and 400-510°C, respectively, the calcination time is 1-2h, and the heating rate is less than 6°C / min;
[0025] Preferably, the calcination in step 2) is performed under a reducing atmosphere, more preferably any one of hydrogen, methane, and carbon monoxide. The calcination in a reducing atmosphere can remove oxidative impurities on the adsorbent surface, and the three-stage calcination can enhance the mechanical strength of the adsorbent.
[0026] An acetylene purification adsorbent prepared according to the method described above.
[0027] The invention discloses an application of an acetylene purification adsorbent prepared according to the method described above in treating acetylene-rich tail gas containing higher alkynes.
[0028] A method for purifying acetylene-rich tail gas, comprising passing acetylene-rich tail gas containing higher alkynes through an acetylene purification adsorbent prepared by the method described above; the adsorption temperature is 0-50°C, preferably 10-30°C; the acetylene-rich tail gas passes through the adsorbent at a space velocity of 200-2000h -1 , preferably 600-800h -1 ;
[0029] Preferably, the higher alkyne is selected from one or more of propadiene and butadiene; more preferably, the propadiene concentration in the acetylene-rich tail gas is ≤10wt%, and the butadiene concentration is ≤8wt%; further preferably, the propadiene concentration in the acetylene-rich tail gas is 2-10wt%, and the butadiene concentration is 0-8wt%.
[0030] The present invention provides an adsorbent for resource utilization, which has enhanced adsorption capacity for higher alkynes (propadiene and butadiene) in acetylene-rich tail gas and can be used for purifying and recovering acetylene in acetylene-rich tail gas. DETAILED DESCRIPTION
[0031] The present invention will be further described below through specific examples. The examples of the present invention are only for illustration of the present invention and do not limit the scope of the present invention.
[0032] The main raw material information in the following examples of the present invention is as follows:
[0033] Acetylene-rich tail gas: contains 55% acetylene, 10% propylene, 15% carbon dioxide, and 20% nitrogen, calculated by volume, and comes from Wanhua Chemical's Sichuan BDO unit.
[0034] Unless otherwise specified, other raw materials and reagents can be purchased from commercial sources.
[0035] The main test equipment used in the following embodiments are:
[0036] The specific surface area was measured using a V-Sorb 2800S specific surface area meter produced by Beijing Jin'ep Technology Co., Ltd.
[0037] The contact angle was measured using an SL200B contact angle tester produced by Shanghai Solon Company;
[0038] The components in the acetylene-rich tail gas were analyzed by gas chromatography external standard method, and the gas chromatograph was Agilent 7890B produced by Agilent.
[0039] [Example 1]
[0040] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0041] 1) Acetylene black (Wanhua Chemical Sichuan) and BDO tar (Wanhua Chemical Sichuan) were weighed and mixed in a mass ratio of 1:1, and heated under a nitrogen atmosphere at 600°C for 8 hours to obtain a porous material;
[0042] 2) The porous material obtained in step 1) was crushed to 400 mesh, immersed in a 10 wt% sodium bicarbonate aqueous solution, and subjected to a modification treatment under 120 Hz ultrasonic conditions for 2 h. After the modification, the solid was filtered out and dried. Basic copper carbonate was weighed in an amount of 1% by weight of the porous material and mixed with the dried solid. The mixture was then calcined in three stages under a hydrogen atmosphere at temperatures of 160° C., 320° C., and 480° C., for 1 h, 2 h, and 2 h, respectively, at a heating rate of 4° C. / min, to produce adsorbent A.
[0043] [Example 2]
[0044] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0045] 1) Acetylene black (Xinjiang Meike) and BDO tar (Wanhua Chemical Sichuan) were weighed and mixed at a mass ratio of 1.2:1, and heated under a nitrogen atmosphere at a temperature of 550°C for 6 h to obtain a porous material;
[0046] 2) The porous material obtained in step 1) was crushed to 350 mesh, immersed in an 8 wt% sodium bicarbonate aqueous solution, and modified under 120 Hz ultrasonic conditions for 2 h. After the modification, the solid was filtered out and dried. Bismuth subcarbonate was weighed according to 3.75% of the mass of the porous material and mixed with the dried solid. The mixture was then calcined in three stages under a hydrogen atmosphere at temperatures of 150° C., 310° C., and 500° C. for 1 h, 2 h, and 2 h, respectively, at a heating rate of 4° C. / min to obtain adsorbent B.
[0047] [Example 3]
[0048] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0049] 1) Acetylene black (Wanhua Chemical Sichuan) and BDO tar (Wanhua Chemical Sichuan) were weighed and mixed at a mass ratio of 0.9:1, and heated under a nitrogen atmosphere at a temperature of 520°C for 7 hours to obtain a porous material;
[0050] 2) The porous material obtained in step 1) was crushed to 400 mesh, immersed in a 5 wt% sodium bicarbonate aqueous solution, and subjected to a modification treatment under 120 Hz ultrasonic conditions for 2 h. After the modification, the solid was filtered out and dried. Basic lead carbonate was weighed to 1.1% of the mass of the porous material and mixed with the dried solid. The mixture was then calcined in three stages under a hydrogen atmosphere at temperatures of 150° C., 310° C., and 500° C., for 1 h, 2 h, and 2 h, respectively, at a heating rate of 4° C. / min, to produce Adsorbent C.
[0051] [Example 4]
[0052] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0053] 1) Acetylene black (Xinjiang Meike) and BDO tar (Xinjiang Meike) were weighed and mixed at a mass ratio of 0.1:1, and heated under a nitrogen atmosphere at a temperature of 500° C. for 3 h to obtain a porous material;
[0054] 2) The porous material obtained in step 1) was crushed to 20 mesh size, immersed in a 1 wt% aqueous sodium bicarbonate solution, and subjected to a modification treatment under 100 Hz ultrasonic conditions for 3 h. After modification, the solid was filtered out and dried. Basic lead carbonate was weighed to 0.5% of the mass of the porous material and mixed with the dried solid. The mixture was then calcined in three stages under a hydrogen atmosphere at temperatures of 120° C., 220° C., and 500° C. for 2 h, 2 h, and 2 h, respectively, at a heating rate of 1° C. / min, to produce adsorbent D.
[0055] [Example 5]
[0056] A method for preparing an acetylene purification adsorbent comprises the following steps:
[0057] 1) Acetylene black (Wanhua Chemical, Sichuan) and BDO tar (Xinjiang Meike) were weighed and mixed in a mass ratio of 10:1, and heated under a nitrogen atmosphere at 800°C for 4 h to obtain a porous material;
[0058] 2) The porous material obtained in step 1) was crushed to 500 mesh, immersed in a 20 wt% sodium bicarbonate aqueous solution, and subjected to modification treatment under 808 Hz ultrasonic conditions for 4 hours. After modification, the solid was filtered out and dried. Basic lead carbonate was weighed to 8% of the mass of the porous material and mixed with the dried solid. The mixture was then calcined in three stages under a hydrogen atmosphere at temperatures of 140° C., 250° C., and 490° C., for 1 hour, 1.5 hours, and 2 hours, respectively, at a heating rate of 6° C. / min, to produce adsorbent E.
[0059] [Comparative Example 1]
[0060] Adsorbent M was prepared in substantially the same manner as in Example 1, except that in step 2), the porous material was not immersed in an aqueous sodium bicarbonate solution.
[0061] [Comparative Example 2]
[0062] Adsorbent N was prepared in substantially the same manner as in Example 1, except that in step 2), basic copper carbonate was not added to the porous material for mixing.
[0063] [Comparative Example 3]
[0064] Adsorbent P was prepared in substantially the same manner as in Example 1, except that the BDO tar in step 1) was replaced with acetylene black of the same mass.
[0065] Application Example 1
[0066] The adsorption performance of the adsorbents prepared in the above examples and comparative examples was studied using the following experimental conditions:
[0067] Before the experiment began, the contact angle, specific surface area, and strength of each adsorbent were measured and recorded in Table 1. Subsequently, the adsorbent was placed in a glass cylindrical adsorption tower (with a jacket, inner diameter of 25 cm, height of 40 cm), and then the acetylene-rich tail gas was passed into the adsorption tower at an air velocity of 300 h -1 The initial adsorption temperature was 25°C, and the outlet tail gas was continuously detected by gas chromatography. The treatment effect of the adsorbent is shown in Table 1.
[0068] Table 1
[0069]
[0070] Note: Propylene breakthrough time is based on the outlet propadiene concentration reaching 5000ppm.
[0071] Application Example 2
[0072] According to the method in Application Example 1, long-term adsorption experiments were conducted on adsorbents A and M, with a total of 40 adsorption cycles. The test results are shown in Table 2. The recycling method of the adsorbents is as follows:
[0073] The saturated adsorbent was taken out and placed in an oven, and heated at a rate of 10°C / 5min. After the temperature reached 120°C, it was stabilized for 3h, and then cooled to room temperature for reuse.
[0074] Table 2
[0075]
[0076]
[0077] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be considered as the scope of protection of the present invention.
Claims
1. A method for preparing an acetylene purification adsorbent, characterized in that: The following steps are involved: 1) After weighing and mixing acetylene carbon black and BDO tar, heat-treating the mixture in an inert atmosphere to obtain a porous material; the weighing ratio of the acetylene carbon black and BDO tar is (0.1-10):1, preferably (0.5-2):1; 2) The porous material obtained in step 1) is crushed and then immersed in a sodium bicarbonate aqueous solution for modification. After the treatment, the solid is filtered out, dried, mixed with a basic metal salt, and calcined to obtain the adsorbent.
2. The method for preparing an acetylene purification adsorbent according to claim 1, characterized in that: In step 1), the temperature of the heating treatment is 300-1000° C., preferably 500-800° C., and the preferred heating treatment time is 1-24 h, preferably 1-3 h; Preferably, the heating treatment is carried out according to a heating-cooling procedure, which is repeated 1-10 times, preferably 1-3 times; Preferably, the inert atmosphere is provided by nitrogen and / or argon.
3. The method for preparing an acetylene purification adsorbent according to claim 1 or 2, characterized in that: The acetylene carbon black is a byproduct carbon black derived from the natural gas process for producing acetylene, and preferably comprises 98-99wt% of inorganic carbon, 1-2wt% of benzene series and higher hydrocarbons above C10; Preferably, the BDO tar is a byproduct tar produced by the acetylene aldehyde process to produce 1,4-butanediol, and preferably comprises 1-25 wt% of 1,4-butanediol, 1-5 wt% of alkali metal salt, and 70-98 wt% of polymer.
4. The method for preparing the acetylene purification adsorbent according to any one of claims 1 to 3, characterized in that: In step 2), the porous material is crushed to 20-500 mesh, preferably 200-400 mesh; Preferably, the concentration of the sodium bicarbonate aqueous solution is 1-20 wt%, preferably 5-10 wt%.
5. The method for preparing the acetylene purification adsorbent according to any one of claims 1 to 4, characterized in that: The modification method in step 2) is ultrasonic treatment for 1-5h.
6. The method for preparing the acetylene purification adsorbent according to any one of claims 1 to 5, characterized in that: In step 2), the amount of the basic metal salt is 0.1-10wt% of the mass of the porous material before modification, preferably 0.5-2wt%; Preferably, the basic metal salt is a basic carbonate selected from any one or more of metal copper, bismuth and lead, preferably one or more of basic copper carbonate, basic bismuth carbonate and basic lead carbonate.
7. The method for preparing an acetylene purification adsorbent according to any one of claims 1 to 6, characterized in that: In step 2), the calcination is a gradient calcination, preferably a three-stage calcination, the first, second and third stage calcination temperatures are 120-170°C, 220-320°C, 400-510°C, the calcination time is 1-2h, and the heating rate is less than 6°C / min; Preferably, the calcination in step 2) is carried out under a reducing atmosphere, and more preferably the reducing atmosphere is any one of hydrogen, methane and carbon monoxide.
8. An acetylene purification adsorbent prepared according to the method according to any one of claims 1 to 7.
9. Use of an acetylene purification adsorbent prepared according to the method according to any one of claims 1 to 7 in treating acetylene-rich tail gas containing higher alkynes.
10. A method for purifying acetylene-rich tail gas, characterized in that: The invention comprises the following steps: passing acetylene-rich tail gas containing higher alkynes through the acetylene purification adsorbent prepared by the method described in any one of claims 1 to 7; the adsorption temperature is 0-50°C, preferably 10-30°C; the acetylene-rich tail gas passes through the adsorbent at a space velocity of 200-2000h -1 , preferably 600-800h -1 ; Preferably, the higher alkyne is selected from one or more of propadiene and butadiene; more preferably, the propadiene concentration in the acetylene-rich tail gas is ≤10wt%, and the butadiene concentration is ≤8wt%; further preferably, the propadiene concentration in the acetylene-rich tail gas is 2-10wt%, and the butadiene concentration is 0-8wt%.
Citation Information
Patent Citations
Method for drying acetylene by adopting adsorbent
CN113956128A
Scale-like copper-based adsorbent as well as preparation method and application thereof
CN115007105A
Method for subtracting hydrocarbor impurities of above C3+ from mixed acetylene gas and recovering acetylene
CN1405129A
Methods and apparatus for stabilizing vanadium compounds
KR1020210132612A