Preparation method of 3D printing molecular sieve catalyst, prepared molecular sieve catalyst and application
By using aluminosilicate and photosensitive resin slurry for sintering and hydrothermal crystallization in 3D printed molecular sieve catalysts, the problems of low molecular sieve content and low accessibility of active centers are solved, achieving efficient catalytic activity and structural precision. , suitable for catalytic cracking reactions.
Patent Information
- Application Number
- CN202310341587.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-31
- Publication Date
- 2024-10-15
AI Technical Summary
Existing 3D printed molecular sieve catalysts have low molecular sieve content and low accessibility of active centers, which cannot meet the needs of practical applications.
Aluminosilicate photosensitive resin slurry containing aluminosilicate and photosensitive resin is used for 3D printing. After sintering, hydrothermal crystallization and roasting, a molecular sieve catalyst is prepared to increase the content of the molecular sieve and the proximity of the active center.
The molecular sieve catalyst has high molecular sieve content, high structural precision, high catalytic activity, reduced bed pressure drop, and is suitable for catalytic cracking reactions.
Smart Images

Figure CN118767974A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of molecular sieve catalysts, and in particular to a method for preparing a 3D printed molecular sieve catalyst and the prepared molecular sieve catalyst and its application. Background Art
[0002] The rapid growth of global chemical market demand has stimulated the vigorous development of catalytic cracking technology to increase the production of low-carbon olefins. In the 1970s, Mobil Corporation developed ZSM-5 molecular sieve, which has straight pores. and sinusoidal pores It has become the most competitive solid acid catalyst with its unique shape-selective catalytic effect and excellent thermal / hydrothermal stability. In practical applications, molecular sieve powder needs to be processed with binder / matrix materials into shaped catalysts such as microspheres, granules or strips before it can be used. The structure, composition and catalytic performance of the shaped catalyst will be quite different from those of the initial molecular sieve powder. Therefore, how to optimize the catalyst forming method to improve the accessibility of the active sites of molecular sieve-based catalysts and improve the reaction performance is an important issue in the research and development and production of molecular sieve catalysts.
[0003] Processing solid powdered catalytic materials into structured catalysts with open pores (such as honeycomb ceramics) will effectively improve their mass transfer / heat transfer capabilities. 3D printing, also known as additive manufacturing, is based on a three-dimensional digital model file, and solidifies ink with a certain flow capacity by stacking layers to achieve material molding of complex geometric shapes. Compared with the traditional extrusion molding method, 3D printing molding technology has the advantages of high precision, multifunctional material integration and digital / flexible design. Up to now, a variety of 3D printed structured catalysts with molecular sieves as the main active components have shown great application potential in alkane catalytic cracking, ethylene oxidation, carbon monoxide oxidation, xylene isomerization and α-pinene isomerization reactions. For example, Stuecker et al. (Industrial & Engineering Chemistry Research, 2005, 44, 302) prepared alternating stacked structured catalysts by extrusion molding 3D printing, which can significantly improve the mass transfer efficiency of carbon monoxide catalytic oxidation reaction and keep the pressure drop loss at a low level. At present, molecular sieves are coated on the surface of 3D printed structured materials by secondary growth, surface deposition or coordination (X. Li, et al, Chemical Engineering Journal 2018, 333, 545; E. et.al,Applied Catalysis A:General 2019,579,75;CYChaparro-Garnica,et.al,ACS Applied Materials&Interfaces 2020,12,54573;A.Lind et.al,Materials&Design 2020,187,108377;X.Li,ACS Applied EnergyMaterials 2018,1,2740), but the above method has the problem that the molecular sieve content in the catalyst is relatively low (no more than 20%) and cannot meet the needs of practical applications (30%-50%). At the same time, the accessibility of the active center of the molecular sieve in the 3D printed regular catalyst needs to be further improved.
[0004] In summary, although the preparation of 3D printed molecular sieve catalysts is currently a hot topic for scientific researchers, the 3D printed molecular sieve catalysts obtained by existing methods have the problems of low molecular sieve content and low accessibility of active centers, which cannot meet application requirements. In view of this, the development of a 3D printed catalyst preparation route with high molecular sieve content and accessible molecular sieve active sites has important practical significance and application value. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of low molecular sieve content and low accessibility of active centers in the prepared 3D printed molecular sieve catalyst in the prior art, and to provide a preparation method of a 3D printed molecular sieve catalyst and the prepared molecular sieve catalyst and application. The preparation method is simple in process, the molecular sieve catalyst has a high molecular sieve content and high catalytic activity.
[0006] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a 3D printed molecular sieve catalyst, the method comprising the following steps:
[0007] (1) providing an aluminosilicate photosensitive resin slurry containing aluminosilicate and a photosensitive resin, and then performing 3D printing to obtain an aluminosilicate ceramic body;
[0008] (2) sintering the aluminosilicate ceramic body to obtain an aluminosilicate ceramic carrier;
[0009] (3) crystallizing a crystallization mother solution containing a silicon source, an aluminum source, a template, an alkali source and water to obtain a crystallization incubation solution;
[0010] (4) hydrothermally crystallizing the aluminosilicate ceramic carrier in a crystallization incubation solution, and then calcining the solid product obtained by the hydrothermal crystallization.
[0011] Preferably, the aluminosilicate comprises silicon-based powder and auxiliary powder, the mass percentage of the silicon-based powder on a dry basis is 35-65%, and the mass percentage of the auxiliary powder on a dry basis is 35-65%.
[0012] The second aspect of the present invention provides a 3D printed molecular sieve catalyst prepared by the preparation method described in the first aspect.
[0013] Preferably, the 3D printed molecular sieve catalyst comprises 30-55% by mass of ZSM-5 molecular sieve.
[0014] Preferably, the ZSM-5 molecular sieve is distributed on the surface of the 3D printed molecular sieve catalyst and exists in the form of micron particle aggregates. Preferably, the average particle size of the micron particles is 1-5 microns.
[0015] Preferably, the micropore volume of the catalyst is 0.04-0.1 cm 3 / g; mesopore volume is 0.05-0.09cm 3 / g.
[0016] The third aspect of the present invention provides an application of the 3D printed molecular sieve catalyst prepared by the method described in the first aspect or the 3D printed molecular sieve catalyst described in the second aspect in a catalytic cracking reaction.
[0017] Through the above technical solution, the present invention has the following advantages:
[0018] (1) The preparation method provided by the present invention can establish a model through three-dimensional software, and can customize complex three-dimensional structures suitable for different scenes. It does not rely on molds, and does not require complex post-processing of the carrier. The three-dimensional pore structure of the carrier is simple and controllable;
[0019] (2) The molecular sieve catalyst prepared by the preparation method provided by the present invention has a high molecular sieve content and high structural accuracy, and the molecular sieve is directly exposed to the outer surface of the carrier through in-situ growth, which has the advantage of high accessibility of the active center;
[0020] (3) In the performance test of the catalytic cracking reaction, the prepared molecular sieve catalyst has high catalytic activity and has the advantage of reducing the bed pressure drop compared with the traditional powder particle molecular sieve catalyst in the present invention, and has application prospects in the field of catalytic cracking in the future;
[0021] (4) In the present invention, the prepared molecular sieve catalyst is easy to separate and recover from the synthesis solution, and the synthesis process has low requirements on equipment. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 is a cross-sectional view of the three-dimensional model test established in Example 1;
[0023] Figure 2 is a photo of the 3D printed molecular sieve catalyst prepared in Example 1;
[0024] Figure 3 is the XRD pattern of the 3D printed molecular sieve catalyst prepared in Example 1;
[0025] Figure 4 is a low-magnification scanning electron microscope image of the 3D printed molecular sieve catalyst prepared in Example 1;
[0026] Figure 5 This is a high-magnification scanning electron microscope image of the 3D printed molecular sieve catalyst prepared in Example 1;
[0027] Figure 6 is the isothermal adsorption curve of the 3D printed molecular sieve catalyst prepared in Example 1;
[0028] Figure 7 is the pore distribution curve of the 3D printed molecular sieve catalyst prepared in Example 1;
[0029] Figure 8 is the XRD pattern of the catalyst prepared in Comparative Example 1;
[0030] Fig. 9 This is a high-magnification scanning electron microscope image of the catalyst prepared in Comparative Example 1. DETAILED DESCRIPTION
[0031] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0032] A first aspect of the present invention provides a method for preparing a 3D printed molecular sieve catalyst, the method comprising the following steps:
[0033] (1) providing an aluminosilicate photosensitive resin slurry containing aluminosilicate and a photosensitive resin, and then performing 3D printing to obtain an aluminosilicate ceramic body;
[0034] (2) sintering the aluminosilicate ceramic body to obtain an aluminosilicate ceramic carrier;
[0035] (3) crystallizing a crystallization mother solution containing a silicon source, an aluminum source, a template, an alkali source and water to obtain a crystallization incubation solution;
[0036] (4) hydrothermally crystallizing the aluminosilicate ceramic carrier in a crystallization incubation solution, and then calcining the solid product obtained by the hydrothermal crystallization.
[0037] In the present invention, the aluminosilicate ceramic carrier is hydrothermally crystallized in a crystallization incubation solution, and a molecular sieve with good dispersibility and high catalytic activity can be obtained on the aluminosilicate ceramic carrier. The preparation process is simple and can form a complex three-dimensional structure without relying on a mold. The prepared molecular sieve catalyst has high structural accuracy, high molecular sieve content in the catalyst, and high catalytic activity.
[0038] In the present invention, preferably, the aluminosilicate photosensitive resin slurry in step (1) can be obtained by mixing aluminosilicate and photosensitive resin. There is no particular limitation on the mixing method. According to a preferred embodiment of the present invention, the mixing can be achieved by ball milling, the ball milling speed is 250-500 rpm, preferably 280-450 rpm, and the ball milling time is 3-18 hours, preferably 5-15 hours.
[0039] According to the present invention, preferably, the aluminosilicate comprises silicon-based powder and auxiliary powder, the mass percentage of silicon-based powder on a dry basis is 35-65%, preferably 45-60%, and the mass percentage of auxiliary powder on a dry basis is 35-65%, preferably 40-55%. The use of such aluminosilicate with such a preferred composition is more conducive to the carrier material obtained after sintering taking into account both structural stability and chemical activity under hydrothermal conditions.
[0040] In the present invention, the aluminosilicate has the conventional meaning in the art. Aluminosilicate is a class of substances including commonly used mineral soils, the main components of which are aluminum oxide and silicon dioxide. The molecular formula can be expressed as xAl2O3·ySiO2, wherein the ratio of aluminum oxide to silicon dioxide is not constant.
[0041] In the present invention, there is no particular limitation on the particle size of the aluminosilicate, which can be larger particles or smaller powders, as long as the aluminosilicate is evenly distributed in the carrier. If larger particles are used, it is preferred to further improve their uniformity through subsequent ball milling. Preferably, the particle size D90 of the aluminosilicate is in the range of 0.5-100 μm.
[0042] In the present invention, preferably, the above-mentioned silicon-based powder is mixed with an auxiliary powder to obtain aluminosilicate, and the silicon-based powder can be used as a silicon source for growing molecular sieves on a carrier in the subsequent preparation process. When the amount of the silicon-based powder added is too much, the silicon dissolution degree of the carrier after calcination during the hydrothermal crystallization process is too high, and the in-situ molecular sieve growth reaction rate on the carrier surface is too high, making the carrier structure unstable and collapsing, and no longer maintaining the original self-supporting structure. When the amount of silicon-based powder added is insufficient, the silicon dissolution of the carrier after calcination during the hydrothermal crystallization process is limited, resulting in a too low in-situ molecular sieve growth reaction rate on the carrier surface, so that the molecular sieve content in the catalyst finally obtained is low, and the catalytic reaction requirements cannot be met.
[0043] In the present invention, there is no particular limitation on the particle sizes of the silicon-based powder and the auxiliary powder. It is preferred that the particle size of the aluminosilicate obtained after mixing meets the above-mentioned particle size requirements.
[0044] According to the present invention, the silicon-based powder may be conventional silicon-based powder in the art, and those skilled in the art can make an adaptive selection according to needs. Preferably, the silicon-based powder is selected from at least one of silicon dioxide, white carbon black and diatomaceous earth.
[0045] According to the present invention, there is no particular limitation on the auxiliary powder, as long as it is chemically inert under hydrothermal conditions to maintain the stability of the self-supporting structure. Preferably, the auxiliary powder is selected from at least one of kaolin, metakaolin, bentonite and montmorillonite.
[0046] According to the present invention, the amount of the aluminosilicate and the photosensitive resin can be selected in a relatively wide range, so as to ensure that the 3D printing process proceeds smoothly. Preferably, the mass ratio of the aluminosilicate to the photosensitive resin is 0.5-1:1, such as 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, and any range between any two values, preferably 0.6-0.9:1.
[0047] According to the present invention, the specific composition of the photosensitive resin has a wide range of selections and can be selected according to conventional technical means in the art. Preferably, the raw materials of the photosensitive resin include 1-5% of photoinitiator, 30-65% of prepolymer, and 30-65% of monomer by mass percentage, preferably including 1.5-4% of photoinitiator, 35-60% of prepolymer, and 37-62% of monomer by mass percentage. The photosensitive resin composed of the above raw materials is used for 3D printing, which has fast curing speed and high production efficiency.
[0048] In the present invention, the photoinitiator can be a conventional photoinitiator in the art. Preferably, the photoinitiator is selected from at least one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (photoinitiator TPO), phenyl bis(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819) and isopropylthioxanthone (ITX).
[0049] In the present invention, the prepolymer may be a conventional acrylate prepolymer in the art. Preferably, the prepolymer is an epoxy acrylate prepolymer and / or a polyurethane acrylate prepolymer.
[0050] In the present invention, the monomer may be a conventional monomer in the art. Preferably, the monomer is selected from at least one of 1,6-hexanediol diacrylate (HDDA), tripropylene glycol diacrylate (TPGDA) and trimethylolpropane triacrylate (TMPTA).
[0051] In the present invention, a 3D printing method is used to prepare an aluminosilicate ceramic body, a modeling software is used to perform a three-dimensional structure design, and an aluminosilicate photosensitive resin slurry is poured into a DLP light-curing printer material cylinder for printing to obtain an aluminosilicate ceramic body. In the present invention, "aluminosilicate ceramic body" is a general term for the prepared bodies, and the printing method can be used to customize complex three-dimensional structures suitable for different scenes, without relying on molds, and does not require complex post-processing of the carrier, and the three-dimensional channel structure of the carrier is simple and controllable.
[0052] In the present invention, preferably, a modeling software is used for three-dimensional structure design, and the modeling software is selected from SolidWorks, 3DMAX, AutoCAD or Materialise Magics.
[0053] According to the present invention, preferably, the conditions for 3D printing include: the light curing exposure power is 0.5-5mW / cm 2 The exposure time of the first layer is 15-30s, the exposure time of other layers is 5-15s, and the thickness of a single layer of photocuring is 20-100μm.
[0054] In the present invention, preferably, the obtained aluminosilicate ceramic body is also cleaned after printing. There is no particular limitation on the cleaning conditions, and those skilled in the art can make appropriate selections. According to a preferred embodiment of the present invention, anhydrous ethanol is used for sufficient cleaning.
[0055] The present invention does not particularly limit the size and structural shape of the aluminosilicate ceramic body, and those skilled in the art can make appropriate selections according to the specific application scenarios of the prepared catalyst. The present invention subsequently provides a specific preferred embodiment for use in a catalytic cracking catalyst, but the present invention is not limited thereto.
[0056] In the present invention, the aluminosilicate ceramic body provides a skeleton for the molecular sieve catalyst. The body has a multi-porous structure and forms an aluminosilicate ceramic carrier after sintering, so that the molecular sieve seeds in the crystallization incubation solution can grow rapidly on the carrier, thereby increasing the mass percentage of the molecular sieve (preferably ZSM-5) in the prepared molecular sieve catalyst.
[0057] According to the present invention, preferably, the aluminosilicate ceramic carrier has a multi-porous self-supporting three-dimensional structure. The present invention has no special limitation on the multi-porous self-supporting three-dimensional structure, which has the conventional interpretation in the art. Specifically, the "self-supporting" means that the aluminosilicate ceramic carrier has its own strength and rigidity, and can maintain its shape and stability without external support. The "multi-porous" means that the main frame of the aluminosilicate ceramic carrier has a multi-porous structure. There is no special limitation on the distribution of the pores, and it can be appropriately selected according to the specific catalyst application scenario. The distribution of the pores can be uniform, symmetrical, or uneven and asymmetrical. In order to further improve the application effect of the catalyst in catalytic cracking reactions, it is further preferred that the aluminosilicate ceramic carrier is a self-supporting three-dimensional structure with parallel radial and axial interconnected pore structures. The specific pore structure is as follows Figure 1 and Figure 2 shown.
[0058] According to the present invention, preferably, the sintering conditions in step (2) include: a temperature of 1100-1300° C. and a time of 5-20 hours. Further preferably, the sintering conditions in step (2) include: a temperature of 1150-1250° C. and a time of 8-16 hours.
[0059] In the present invention, the aluminosilicate ceramic body is sintered in step (2), and those skilled in the art can adjust the heating rate of the sintering process as needed. Preferably, the heating rate is 0.1-10°C / min, preferably 0.5-5°C / min.
[0060] According to the present invention, preferably, the method also includes pyrolyzing the aluminosilicate ceramic body before sintering to remove organic matter in the body, and the pyrolysis conditions include: temperature of 350-550°C and time of 5-15h; preferably, the pyrolysis conditions include: temperature of 380-520°C and time of 6-13h.
[0061] In the present invention, those skilled in the art can adjust the heating rate of the pyrolysis process as needed. Preferably, the heating rate of the pyrolysis process is 0.1-5°C / min, preferably 0.5-2°C / min.
[0062] According to the present invention, preferably, in the crystallization mother solution, the aluminum source is calculated as Al2O3, the silicon source is calculated as SiO2, the alkali source is calculated as Na2O, and the molar ratio of SiO2:Al2O3:template:Na2O:H2O is 1:(0.003-0.03):(0.05-0.25):(0.05-0.3):(30-55), preferably 1:(0.005-0.025):(0.08-0.2):(0.08-0.25):(35-50).
[0063] In the present invention, preferably, the silicon source, aluminum source and template are used to provide molecular sieve seeds for the crystallization mother solution, which helps to accelerate the growth rate of the molecular sieve on the aluminosilicate ceramic carrier and shorten the crystallization time of the molecular sieve.
[0064] According to the present invention, preferably, the silicon source may be a conventional silicon source in the art, and those skilled in the art may make an adaptive selection according to needs, preferably silica sol and / or tetraethyl orthosilicate.
[0065] According to the present invention, preferably, the aluminum source can be a conventional aluminum source in the art, and those skilled in the art can make an adaptive selection as needed, preferably selected from at least one of aluminum sulfate, aluminum isopropoxide and aluminum trichloride.
[0066] In the present invention, the template agent has a wide selection range and can be adaptively selected according to the specific type of molecular sieve to be synthesized. Preferably, the template agent is an organic amine microporous template agent known to those skilled in the art that can be used to prepare ZSM-5, preferably tetrapropylammonium hydroxide and / or tetrapropylammonium bromide.
[0067] According to the present invention, preferably, the crystallization conditions in step (3) include: a crystallization temperature of 155-185° C., preferably 165-180° C., and a crystallization time of 3-10 h, preferably 4-9 h.
[0068] In the present invention, the reaction equipment for the crystallization and hydrothermal crystallization has a wide range of options, and those skilled in the art can make adaptive choices as needed, preferably in a crystallization kettle. In the present invention, it is preferred that after the crystallization and / or hydrothermal crystallization is completed, the crystallization kettle is cooled (preferably to room temperature) and then opened. This preferred embodiment avoids the safety hazard when the kettle is opened due to the self-generated pressure in the kettle caused by the crystallization reaction at high temperature.
[0069] In the present invention, preferably, the crystallization mother liquor is crystallized under the above conditions to obtain a crystallization incubation solution, which can further improve the crystallinity of the prepared molecular sieve catalyst. The crystallization incubation solution contains molecular sieve seeds. From the perspective of crystal growth kinetics, the use of the incubation solution can significantly shorten the crystal nucleation period (nucleation period) on the carrier surface, thereby accelerating the molecular sieve crystallization process on the carrier surface.
[0070] According to the present invention, preferably, in step (4), the mass ratio of the aluminosilicate ceramic carrier to the crystallization incubation solution is 1:6-20, such as 1:6, 1:7, 1:8, 1:9, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, and any range between any two values, preferably 1:8-15. This preferred embodiment is more conducive to matching the dissolution rate of the silicon species of the carrier itself and the crystallization rate of the surface molecular sieve, and obtaining a crystallized product that takes into account both crystallinity and self-supporting structural strength.
[0071] According to the present invention, preferably, the conditions for the hydrothermal crystallization include: a crystallization temperature of 155-185° C., preferably 165-180° C., and a crystallization time of 12-40 h, preferably 15-35 h.
[0072] In the present invention, preferably, the method further comprises: post-processing the solid product obtained by hydrothermal crystallization, wherein the post-processing comprises washing and drying. The washing may be performed by conventional methods and conditions in the art, and according to some preferred embodiments of the present invention, the washing may be performed by deionized water.
[0073] In the present invention, drying can be carried out by conventional methods and conditions in the art. According to some preferred embodiments of the present invention, drying can be carried out in an oven under the conditions of: drying at 60-120° C. for 2-10 hours.
[0074] According to the present invention, there is no particular limitation on the conditions for the calcination, as long as the template in the solid product can be removed. Preferably, the calcination conditions include: a temperature of 500-600°C and a time of 4-8 hours. There is no particular limitation on the calcination equipment. Preferably, the calcination can be carried out in a muffle furnace.
[0075] According to the present invention, preferably, in the 3D printed molecular sieve catalyst prepared by the method, the mass percentage of ZSM-5 molecular sieve is 30-55%, preferably 35-52%.
[0076] In the present invention, the mass percentage of the molecular sieve in the molecular sieve catalyst is expressed by relative crystallinity, and with reference to ASTM D3906-03 standard, commercial ZSM-5 molecular sieve is used as the standard (Tianjin Nanhua Catalyst Co., Ltd., Na-type ZSM-5 molecular sieve of Nankai University Catalyst Factory, silicon-aluminum ratio 25), and the commercial ZSM-5 crystallinity is defined as 100%. The ratio of the characteristic peak area of the 2θ angle between 22.0-25.0° and the characteristic peak area of the standard molecular sieve in the XRD spectrum of the crystallized product is defined as relative crystallinity. Test instrument: D5005 X-ray diffractometer of Siemens, Germany. Test conditions: Cu target, Kα radiation, solid detector, tube voltage 40kV, tube current 40mA, step scan, step width 0.02°, prefabrication time 2s, scanning range 5°-70°.
[0077] The second aspect of the present invention provides a 3D printed molecular sieve catalyst prepared by the preparation method described in the first aspect.
[0078] According to the present invention, preferably, the 3D printed molecular sieve catalyst comprises 30-55% by mass of ZSM-5 molecular sieve, and further preferably, the 3D printed molecular sieve catalyst comprises 35-52% by mass of ZSM-5 molecular sieve.
[0079] According to the present invention, preferably, the ZSM-5 molecular sieve is distributed on the surface of the 3D printed molecular sieve catalyst and exists in the form of micron particle aggregates. Preferably, the average particle size of the micron particles is 1-5 microns, and more preferably 1.5-4 microns.
[0080] In the present invention, the average particle size of the molecular sieve catalyst is tested in an electron microscope (Hitachi scanning electron microscope, S-4800), and the average value is obtained by randomly measuring the sizes of 20 molecular sieve grains through Nano Measurer software. In the measurement process, the size of a molecular sieve grain is the straight-line distance obtained by connecting the two farthest end points on the particle in the electron microscopic image.
[0081] According to the present invention, preferably, the micropore volume of the catalyst is 0.04-0.1 cm 3 / g, preferably 0.05-0.09cm 3 / g; mesopore volume is 0.05-0.09cm 3 / g, preferably 0.06-0.08cm 3 / g.
[0082] In the present invention, the mesoporous surface area and specific surface area, pore volume (total pore volume) and pore size distribution of the molecular sieve catalyst are measured by low temperature nitrogen adsorption capacity method, and the test instrument is ASAP2400 static nitrogen adsorption instrument of Micromeritics. Test conditions: the sample is vacuum degassed at 1.33Pa and 300°C for 4h, and then contacted with liquid nitrogen at 77K, isothermally adsorbed and desorbed, adsorption and desorption isotherms are measured, and the specific surface area and pore volume are calculated using the BET formula, and the average pore size is calculated using the BJH formula.
[0083] In the present invention, the prepared molecular sieve catalyst has high molecular sieve content and high structural accuracy, and the ZSM-5 molecular sieve is directly exposed to the outer surface of the carrier through in-situ growth, which has the advantage of high accessibility of active centers.
[0084] The third aspect of the present invention provides an application of the 3D printed molecular sieve catalyst prepared by the method described in the first aspect or the 3D printed molecular sieve catalyst described in the second aspect in a catalytic cracking reaction.
[0085] In the present invention, preferably, before the prepared molecular sieve catalyst is used for catalytic cracking reaction, it is pretreated, preferably specifically comprising: exchanging the prepared 3D printed molecular sieve catalyst with ammonia to obtain an ammonia-type catalyst, and then washing, drying and calcining the ammonia-type catalyst to obtain a hydrogen-type catalyst for catalytic cracking experiment. For the above pretreatment conditions, those skilled in the art can make adaptive selections and adjustments as needed.
[0086] In the present invention, preferably, the reaction conditions of the catalytic cracking reaction are: reaction pressure of 0.09-0.3 MPa, reaction temperature of 550-680°C, raw material feed weight space velocity of 50-100h -1 .
[0087] In the present invention, there is no particular limitation on the reaction device for the catalytic cracking reaction, and those skilled in the art can make an appropriate selection according to the application scenario of the molecular sieve catalyst. According to a preferred embodiment of the present invention, the catalytic cracking reaction can be carried out in a fixed bed reactor.
[0088] In the present invention, the prepared molecular sieve catalyst has high catalytic activity and has the advantage of reducing bed pressure drop, and can be widely used in catalytic cracking reactions.
[0089] According to a particularly preferred embodiment of the present invention, a method for preparing a 3D printed molecular sieve catalyst comprises the following steps:
[0090] (1) providing an aluminosilicate photosensitive resin slurry containing aluminosilicate and a photosensitive resin, wherein the aluminosilicate comprises 45-60% of silicon-based powder and 40-55% of auxiliary powder in weight percentage on a dry basis, and the mass ratio of the aluminosilicate to the photosensitive resin is 0.6-0.9:1, and performing 3D printing on the aluminosilicate photosensitive resin slurry to obtain an aluminosilicate ceramic body;
[0091] (2) sintering the aluminosilicate ceramic body at a sintering temperature of 1150-1250° C. for 8-16 hours to obtain an aluminosilicate ceramic carrier;
[0092] (3) crystallizing a crystallization mother solution containing a silicon source, an aluminum source, a template, an alkali source and water, wherein the molar ratio of SiO2:Al2O3:template:Na2O:H2O in the crystallization mother solution is 1:(0.005-0.025):
[0093] (0.08-0.2): (0.08-0.25): (35-50), the crystallization conditions include: a crystallization temperature of 165-180° C., a crystallization time of 4-9 h, and a crystallization incubation solution;
[0094] (4) The aluminosilicate ceramic carrier is hydrothermally crystallized in a crystallization incubation solution, wherein the conditions for the hydrothermal crystallization include: a crystallization temperature of 165-180°C and a crystallization time of 15-35 hours; and then the solid product obtained by the hydrothermal crystallization is calcined, wherein the conditions for the calcination include: a temperature of 500-600°C and a time of 4-8 hours, to obtain a molecular sieve catalyst.
[0095] The present invention will be described in detail below through examples and comparative examples. In the following examples and comparative examples, unless otherwise specified, the reagents and materials used can be obtained commercially, and the room temperature is 25°C;
[0096] The ball milling was carried out using a Juchuang environmental protection vertical planetary ball mill (model JC-QM-0.4);
[0097] The three-dimensional model is established by Solidworks software;
[0098] The 3D printing is completed by a sinking DLP-3D printer (model SU136A or SU-100A) of Foshan Guanglei Intelligent Manufacturing Co., Ltd. (light source wavelength: 405nm);
[0099] The test methods and test conditions for the properties of the molecular sieve catalyst, such as the mass percentage of the molecular sieve, the surface morphology, the average particle size and the pore structure, are described in the aforementioned specification and will not be repeated here.
[0100] Example 1
[0101] (1) Preparation of aluminosilicate ceramic body:
[0102] (1-1) Using diatomite as a silicon-based powder and metakaolin as an auxiliary powder, the silicon-based powder mass fraction is 60% (on a dry basis) and the auxiliary powder mass fraction is 40% (on a dry basis) to obtain aluminosilicate, wherein the D90 particle size of the aluminosilicate is 5.8 μm;
[0103] (1-2) 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) is used as a photoinitiator, polyurethane acrylate prepolymer is used as a prepolymer, and 1,6-hexanediol diacrylate (HDDA) is used as a monomer, and the mixture is mixed according to the ratio of 4% of the photoinitiator, 35% of the prepolymer, and 61% of the monomer to obtain a photosensitive resin;
[0104] (1-3) mixing aluminosilicate and photosensitive resin in a mass ratio of 0.65:1, and fully ball milling in a ball mill for 14 hours (rotation speed 280 rpm) to obtain aluminosilicate photosensitive resin slurry;
[0105] (1-4) Perform three-dimensional structure design, import the three-dimensional model file into the 3D printing equipment, pour the aluminosilicate photosensitive resin slurry into the DLP light-curing printer material tank for printing, and the printing parameters are: exposure power 1mW / cm 2 , exposure time 10s (first layer exposure time 20s); after printing, the obtained aluminosilicate ceramic body is placed in anhydrous ethanol for thorough cleaning.
[0106] (2) drying the formed aluminosilicate ceramic body, and pyrolyzing and sintering the body. The specific pyrolysis and sintering conditions are: heating from room temperature to 450°C at a rate of 0.5°C / min, and maintaining for 8 hours; heating from 450°C to 1200°C at a rate of 3°C / min, and maintaining for 15 hours, to obtain an aluminosilicate ceramic carrier. The aluminosilicate ceramic carrier has Figure 1 A similar multi-porous self-supporting three-dimensional structure is a cylinder composed of strips arranged in a staggered manner horizontally and vertically, with a cross-sectional diameter of 1.26 cm and a height of 0.95 cm. The spacing between different strips on the same horizontal plane is 0.06 cm.
[0107] (3) Using silica sol (40wt% SiO2, Qingdao Junqiang New Materials Co., Ltd.) and aluminum sulfate (99wt%, Innochem) as the silicon source and aluminum source, respectively, and tetrapropylammonium hydroxide (TPAOH, 25wt%, Innochem) as the template, the silicon source, aluminum source, template and sodium hydroxide are added into water and mixed to obtain a crystallization mother solution, wherein the molar ratio of each raw material, i.e., SiO2:Al2O3:template:Na2O:H2O, is 1:0.025:0.1:0.25:35. The above mixture is crystallized at 165°C for 9 hours to obtain a crystallization incubation solution.
[0108] (4) placing the aluminosilicate ceramic carrier in a crystallization incubation solution, wherein the carrier:crystallization incubation solution mass ratio is 1:14, and hydrothermally crystallizing the carrier-incubation solution mixture at 165°C for 35 hours. After the hydrothermal crystallization is completed, the hydrothermal crystallization product is cooled, separated, washed, dried at 100°C for 4 hours, and calcined at 550°C for 5 hours to obtain a 3D printed molecular sieve catalyst.
[0109] Figure 1 This is a test cross-sectional diagram of the three-dimensional model established in Example 1. The three-dimensional structure design is performed by modeling software, and the structural shape of the molecular sieve catalyst can be selected according to actual needs. Figure 2 This is a photo of the 3D printed molecular sieve catalyst prepared in Example 1. The molecular sieve catalyst obtained by 3D printing realizes high-precision, digital design of the molecular sieve catalyst and has better regularity.
[0110] The XRD spectrum of the catalyst prepared in Example 1 is as follows: Figure 3 As shown, from Figure 3 It can be seen that the synthesized 3D printed molecular sieve catalyst has the characteristic diffraction peaks of ZSM-5 molecular sieve, and an obvious five-finger diffraction peak appears at 22.0-25.0° at 2θ. Figure 4 , Figure 5 The low-power scanning electron microscope images and high-power scanning electron microscope images of the catalyst of Example 1 are shown respectively. It can be seen from the figure that the outer surface of the catalyst is densely distributed with ZSM-5 molecular sieve particles, which mainly exist in the form of micron particle aggregates, and the average particle size is 1.6 microns. From the scanning electron microscope image of Example 1, it can be observed that the ZSM-5 molecular sieve is directly exposed to the outer surface of the carrier through in-situ growth, which has the advantage of high accessibility of the active center.
[0111] Figure 6 is the isothermal adsorption curve of the 3D printed molecular sieve catalyst prepared in Example 1, Figure 7 is the pore distribution curve of the 3D printed molecular sieve catalyst prepared in Example 1, such as Figure 6 , Figure 7As shown, a hysteresis loop can be observed in the adsorption isotherm of the 3D printed molecular sieve catalyst, and the presence of mesopores in the sample can be observed from the pore size distribution curve.
[0112] Comparative Example 1
[0113] The 3D printed molecular sieve catalyst was prepared according to the method of Example 1, except that in step (1), no silicon-based powder was used, and all auxiliary powders (kaolin) were used to prepare aluminosilicate to prepare the 3D printed molecular sieve catalyst sample.
[0114] The XRD spectrum of the sample of Comparative Example 1 is as follows: Figure 8 As shown in the figure, it can be seen that the obtained molecular sieve catalyst does not have the characteristic diffraction peak of ZSM-5 molecular sieve, and no obvious five-finger diffraction peak appears at 22.0-25.0°. The SEM image of the sample of Comparative Example 1 is as follows Fig. 9 As shown in the figure, it can be seen that no molecular sieve grains were observed on the surface of the obtained molecular sieve catalyst, and only aluminosilicate particles were observed.
[0115] Comparative Example 2
[0116] A 3D printed molecular sieve catalyst was prepared according to the method of Example 1, except that no crystallization incubation solution was used. Instead, the carrier was directly placed in a crystallization mother liquor for hydrothermal crystallization. The mass ratio of the carrier to the crystallization mother liquor was 1:14, and a 3D printed molecular sieve catalyst sample was prepared.
[0117] Comparative Example 3
[0118] The hydrogen ZSM-5 powder was tableted to prepare 40-60 mesh molecular sieve particles, which were directly used for the evaluation of catalytic cracking of alkane molecules. Except for the different catalysts, other reaction evaluation conditions were the same as those in Example 1.
[0119] Example 2
[0120] (1) Preparation of aluminosilicate ceramic body:
[0121] (1-1) using silicon dioxide as a silicon-based powder and kaolin as an auxiliary powder, the silicon-based powder is mixed at a mass fraction of 50% (on a dry basis) and the auxiliary powder is mixed at a mass fraction of 50% (on a dry basis) to obtain aluminosilicate, wherein the D90 particle size of the aluminosilicate is 25.7 μm;
[0122] (1-2) using phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (819) as a photoinitiator, using polyurethane acrylate prepolymer as a prepolymer, and using tripropylene glycol diacrylate (TPGDA) as a monomer, the mixture is mixed at a ratio of 3% of the photoinitiator, 45% of the prepolymer, and 52% of the monomer to obtain a photosensitive resin;
[0123] (1-3) mixing aluminosilicate and photosensitive resin in a mass ratio of 0.72:1, and fully ball milling in a ball mill for 10 h (rotation speed 350 rpm) to obtain aluminosilicate photosensitive resin slurry;
[0124] (1-4) Perform 3D structure design, import the 3D model file into the 3D printing device, perform 3D printing according to the 3D model of Example 1, pour the aluminosilicate photosensitive resin slurry into the DLP light-curing printer material tank for printing, and the printing parameters are: exposure power 1mW / cm 2 , exposure time 10s (first layer exposure time 20s); after printing, the obtained aluminosilicate ceramic body is placed in anhydrous ethanol for thorough cleaning.
[0125] (2) The formed aluminosilicate ceramic body is dried, pyrolyzed and sintered. The specific pyrolysis and sintering conditions are: heating from room temperature to 500°C at a heating rate of 0.5°C / min and maintaining for 6 hours; heating from 500°C to 1200°C at a heating rate of 3°C / min and maintaining for 10 hours to obtain an aluminosilicate ceramic carrier.
[0126] (3) Using silica sol (40wt% SiO2, Qingdao Junqiang New Materials Co., Ltd.) and aluminum sulfate (99wt%, Innochem) as the silicon source and aluminum source, respectively, and tetrapropylammonium hydroxide (TPAOH, 25wt%, Innochem) as the template, the silicon source, aluminum source, template and sodium hydroxide are added into water and mixed to obtain a crystallization mother solution, wherein the molar ratio of each raw material, i.e., SiO2:Al2O3:template:Na2O:H2O, is 1:0.01:0.1:0.2:40. The above mixture is crystallized at 170°C for 7 hours to obtain a crystallization incubation solution.
[0127] (4) placing the aluminosilicate ceramic carrier in a crystallization incubation solution, wherein the carrier: crystallization incubation solution mass ratio is 1:10, and hydrothermally crystallizing the carrier and crystallization incubation solution mixture at 170°C for 24 hours. After the hydrothermal crystallization is completed, the hydrothermal crystallization product is cooled, separated, washed, dried at 100°C for 4 hours, and calcined at 550°C for 5 hours to obtain a 3D printed molecular sieve catalyst.
[0128] Example 3
[0129] (1) Preparation of aluminosilicate ceramic body:
[0130] (1-1) Using white carbon as a silicon-based powder and bentonite as an auxiliary powder, the mass fraction of the silicon-based powder is 40% (on a dry basis) and the mass fraction of the auxiliary powder is 60% (on a dry basis) to obtain aluminosilicate, wherein the D90 particle size of the aluminosilicate is 85.2 μm;
[0131] (1-2) using isopropylthioxanthone (ITX) as a photoinitiator, using polyurethane acrylate prepolymer as a prepolymer, and using trimethylolpropane triacrylate (TMPTA) as a monomer, the mixture is mixed according to the ratio of 1.5% of the photoinitiator, 60% of the prepolymer, and 38.5% of the monomer to obtain a photosensitive resin;
[0132] (1-3) mixing aluminosilicate and photosensitive resin in a mass ratio of 0.85:1, and fully ball milling in a ball mill for 8 h (rotation speed 400 rpm) to obtain aluminosilicate photosensitive resin slurry;
[0133] (1-4) Perform 3D structure design, import the 3D model file into the 3D printing device, perform 3D printing according to the 3D model of Example 1, pour the aluminosilicate photosensitive resin slurry into the DLP light-curing printer material tank for printing, and the printing parameters are: exposure power 1mW / cm 2 , exposure time 10s (first layer exposure time 20s); after printing, the obtained aluminosilicate ceramic body is placed in anhydrous ethanol for thorough cleaning.
[0134] (2) The formed aluminosilicate ceramic body is dried, pyrolyzed and sintered. The specific conditions are: heating from room temperature to 500°C at a heating rate of 0.5°C / min and maintaining for 6 hours; heating from 500°C to 1200°C at a heating rate of 3°C / min and maintaining for 10 hours to obtain an aluminosilicate ceramic carrier.
[0135] (3) Silica sol (40wt% SiO2, Qingdao Junqiang New Materials Co., Ltd.) and aluminum sulfate (99wt%, Innochem) were used as silicon source and aluminum source, respectively, and tetrapropylammonium hydroxide (TPAOH, 25wt%, Innochem) was used as template. The silicon source, aluminum source, template and sodium hydroxide were added to water and mixed to obtain a crystallization mother solution, wherein the molar ratio of each raw material, i.e., SiO2:Al2O3:template:Na2O:H2O, was 1:0.005:0.15:0.1:45. The above mixture was crystallized at 180°C for 4.5 hours to obtain a crystallization incubation solution.
[0136] (4) The aluminosilicate ceramic carrier is placed in a crystallization incubation solution, wherein the mass ratio of the carrier to the crystallization incubation solution is 1:6, and the carrier and the incubation solution mixture is hydrothermally crystallized at 180°C for 15 hours. After the crystallization is completed, the crystallized product is cooled, separated, washed, dried at 100°C for 4 hours, and calcined at 550°C for 5 hours to obtain a 3D printed molecular sieve catalyst sample.
[0137] Example 4
[0138] A 3D printed molecular sieve catalyst was prepared according to the method of Example 1, except that in step (2), the raw materials in the crystallization mother solution were mixed in a molar ratio of SiO2:Al2O3:template:Na2O:H2O=1:0.005:0.01:0.1:45 to prepare a 3D printed molecular sieve catalyst sample.
[0139] Example 5
[0140] A 3D printed molecular sieve catalyst was prepared according to the method of Example 1, except that the mass percentage of the silicon-based powder on a dry basis was 40%, and the mass percentage of the auxiliary powder on a dry basis was 60%, to obtain a 3D printed molecular sieve catalyst sample.
[0141] Example 6
[0142] A 3D printed molecular sieve catalyst was prepared according to the method of Example 1, except that in step (4), the mass ratio of the carrier to the crystallization incubation solution was 1:7, thereby obtaining a 3D printed molecular sieve catalyst.
[0143] Test Example 1
[0144] The mass percentage of ZSM-5, the particle size of the molecular sieve, and the micropore volume and mesopore volume of the 3D printed molecular sieve catalysts prepared in the examples and comparative examples are shown in Table 1.
[0145] Table 1 Properties of the molecular sieve samples obtained in the examples and comparative examples
[0146]
[0147] As can be seen from Table 1, the 3D printed molecular sieve catalyst prepared in the embodiment has a high mass percentage of ZSM-5 and a high structural accuracy.
[0148] Test Example 2
[0149] Catalytic activity test of 3D printed molecular sieve catalyst.
[0150] First, the prepared 3D printed molecular sieve catalyst was placed in a 0.1 g / mL ammonium sulfate aqueous solution (catalyst: ammonium sulfate mass ratio = 2:1), stirred at 80°C for 2 hours for ion exchange, and exchanged twice in total to obtain an ammonia-type catalyst. The ammonia-type catalyst was then washed, dried, and calcined at 550°C for 4 hours to obtain a hydrogen-type catalyst for catalytic cracking experiments.
[0151] The pretreated 3D printed molecular sieve catalyst was placed in a fixed bed reactor with a reaction pressure of 0.09-0.3 MPa, a reaction temperature of 675 °C, and a feed weight hourly space velocity (WHSV) of 65, 90, and 150 h -1After the reaction, the liquid phase was collected by cooling, and the gas phase product was collected by draining gas collection method. The liquid phase product was analyzed by Agilent 7890B (HP-PONA column) chromatography, and the gas phase product was analyzed by Agilent 6890 chromatography.
[0152] The n-octane conversion rate was calculated according to the following formula: conversion rate = 1-(mass of n-octane in the liquid product / mass of n-octane raw material). The results are shown in Table 2.
[0153] Table 2 Conversion rate of samples obtained from various examples and comparative examples in catalytic cracking reaction of n-octane
[0154]
[0155] Note: Conditions 1, 2, and 3 in Table 2 represent WHSV = 65, 90, and 150h respectively -1 , the reaction temperature is 675℃.
[0156] As can be seen from Table 2, the 3D printed molecular sieve catalysts prepared in Examples 1-3 were used for catalytic cracking reactions, and the conversion rate was significantly higher than that of Comparative Examples 1-2 under the same reaction conditions, and had a better cracking effect on hydrocarbon molecules.
[0157] The catalytic cracking reaction was carried out using the pure molecular sieve particle catalyst of Comparative Example 3, and the conversion rate was significantly lower than that of the embodiment under the same reaction conditions.
[0158] Compared with traditional molecular sieve powder, the 3D printed ZSM-5 molecular sieve catalyst prepared by the present invention is easy to separate and recover from the synthetic solution, the synthesis process has low equipment requirements, and has high catalytic activity. Therefore, the present invention has a good application prospect.
[0159] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for preparing a 3D printed molecular sieve catalyst, characterized in that: The method comprises the following steps: (1) providing an aluminosilicate photosensitive resin slurry containing aluminosilicate and a photosensitive resin, and then performing 3D printing to obtain an aluminosilicate ceramic body; (2) sintering the aluminosilicate ceramic body to obtain an aluminosilicate ceramic carrier; (3) crystallizing a crystallization mother solution containing a silicon source, an aluminum source, a template, an alkali source and water to obtain a crystallization incubation solution; (4) hydrothermally crystallizing the aluminosilicate ceramic carrier in a crystallization incubation solution, and then calcining the solid product obtained by the hydrothermal crystallization.
2. The method according to claim 1, wherein: The aluminosilicate comprises silicon-based powder and auxiliary powder, wherein the mass percentage of silicon-based powder on a dry basis is 35-65%, preferably 45-60%, and the mass percentage of auxiliary powder on a dry basis is 35-65%, preferably 40-55%; Preferably, the silicon-based powder is selected from at least one of silicon dioxide, white carbon black and diatomaceous earth; Preferably, the auxiliary powder is selected from at least one of kaolin, metakaolin, bentonite and montmorillonite.
3. The method according to claim 1 or 2, wherein: The mass ratio of the aluminosilicate to the photosensitive resin is 0.5-1:1, preferably 0.6-0.9:1; Preferably, the raw materials of the photosensitive resin include 1-5% of photoinitiator, 30-65% of prepolymer, and 30-65% of monomer by mass percentage, preferably include 1.5-4% of photoinitiator, 35-60% of prepolymer, and 37-62% of monomer by mass percentage; Preferably, the photoinitiator is selected from at least one of 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and isopropylthioxanthone; Preferably, the prepolymer is an epoxy acrylate prepolymer and / or a polyurethane acrylate prepolymer; Preferably, the monomer is selected from at least one of 1,6-hexanediol diacrylate, tripropylene glycol diacrylate and trimethylolpropane triacrylate.
4. The method according to any one of claims 1 to 3, wherein: The conditions for 3D printing include: the light curing exposure power is 0.5-5mW / cm 2 , the exposure time of the first layer is 15-30s, the exposure time of other layers is 5-15s, and the thickness of a single layer of light curing is 20-100μm; Preferably, the aluminosilicate ceramic carrier has a multi-porous self-supporting three-dimensional structure, and more preferably has a self-supporting three-dimensional structure with parallel radial and axial interconnected pores.
5. The method according to any one of claims 1 to 4, wherein: The sintering conditions in step (2) include: a temperature of 1100-1300° C. and a time of 5-20 hours; Preferably, the method further comprises pyrolyzing the aluminosilicate ceramic body before sintering, and the pyrolysis conditions include: temperature of 350-550° C. and time of 5-15 hours.
6. The method according to any one of claims 1 to 5, wherein: In the crystallization mother solution, the aluminum source is calculated as Al2O3, the silicon source is calculated as SiO2, and the alkali source is calculated as Na2O, and the molar ratio of SiO2:Al2O3:template:Na2O:H2O is 1:(0.003-0.03):(0.05-0.25):(0.05-0.3):(30-55), preferably 1:(0.005-0.025):(0.08-0.2):(0.08-0.25):(35-50); Preferably, the silicon source is silica sol and / or tetraethyl orthosilicate; and / or, the aluminum source is selected from at least one of aluminum sulfate, aluminum isopropoxide and aluminum trichloride; and / or, the template is an organic amine microporous template for preparing ZSM-5.
7. The method according to any one of claims 1 to 6, wherein: The crystallization conditions in step (3) include: a crystallization temperature of 155-185° C., preferably 165-180° C., and a crystallization time of 3-10 h, preferably 4-9 h.
8. The method according to any one of claims 1 to 7, wherein: In step (4), the mass ratio of the aluminosilicate ceramic carrier to the crystallization incubation solution is 1:6-20, preferably 1:8-15, based on their respective total mass; Preferably, the conditions of the hydrothermal crystallization include: a crystallization temperature of 155-185°C, preferably 165-180°C, a crystallization time of 12-40h, preferably 15-35h; Preferably, the calcination conditions include: a temperature of 500-600° C. and a time of 4-8 hours.
9. The method according to any one of claims 1 to 8, wherein: In the 3D printed molecular sieve catalyst prepared by the method, the mass percentage of ZSM-5 molecular sieve is 30-55%.
10. A 3D printed molecular sieve catalyst prepared by the preparation method according to any one of claims 1 to 9; Preferably, the 3D printed molecular sieve catalyst comprises 30-55% by mass of ZSM-5 molecular sieve; Preferably, the ZSM-5 molecular sieve is distributed on the surface of the 3D printed molecular sieve catalyst and exists in the form of micron particle aggregates, and preferably the average particle size of the micron particles is 1-5 microns; Preferably, the micropore volume of the catalyst is 0.04-0.1 cm 3 / g; mesopore volume is 0.05-0.09cm 3 / g.
11. Use of the 3D printed molecular sieve catalyst prepared by the method according to any one of claims 1 to 9 or the 3D printed molecular sieve catalyst according to claim 10 in catalytic cracking reactions.
Citation Information
Patent Citations
Molecular sieve catalyst for catalytic cracking of MTP (methanol to propylene) by-product hydrocarbons and preparation method of molecular sieve catalyst
CN106669790A
Integral molecular sieve catalyst and preparation method and application thereof
CN108620121A
Method for preparing structured catalyst carrier through photocuring
CN111760596A