Method for removing carbonized adhesive film of aviation blade laser drilling protective adhesive tape
By using removers and heat treatment on aviation blades, combined with ultrasonic waves and mechanical stirring, the problem of difficult and incomplete carbonized film removal in the existing technology has been solved, and rapid and efficient carbonized film removal has been achieved, ensuring the integrity of the blades. Completeness and accuracy of fluoroscopy.
Patent Information
- Application Number
- CN202410899981.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
AI Technical Summary
The existing technology is difficult, time-consuming and cannot be completely removed when removing the carbonized film of protective tape after laser drilling of aviation blades, which affects the safety and performance of fluorescence inspection and engines.
The pre-treated aviation blades are soaked in the remover, ultrasonic or mechanically stirred, and heated to 60°C to 90°C. They are then cleaned with acetone or non-halogenated organic solvents and dried with compressed air, and finally dried in an oven. , to ensure the complete removal of the carbonized film.
It achieves rapid, efficient and complete removal of the carbonized film, reduces personnel labor intensity, avoids damage to the blade base, and ensures the accuracy of fluorescence inspection and the safety performance of the engine.
Smart Images

Figure CN118768295A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of processing and protecting high-pressure turbine blades of aircraft engines, and in particular relates to a method for removing a carbonized adhesive film of a protective adhesive tape for laser punching of aircraft blades. Background Art
[0002] In the manufacturing process of aircraft engines, laser drilling is often required for the edge plate and blade body of high-pressure turbine blades. In this process, in order to prevent the blade body from being damaged by the laser and the splashing objects from damaging the blade body, it is usually necessary to use a specific protective tape to protect the blade body. However, due to the high speed and high temperature characteristics of the laser, the film of the protective tape often carbonizes.
[0003] The formation of carbonized film not only affects the surface quality after laser drilling, but also seriously interferes with the subsequent fluorescent inspection work. The carbonized film will distort the results of the fluorescent inspection and may cause potential blade defects to be concealed, thus affecting the safety and performance of the engine.
[0004] At present, the commonly used method in the industry is to soak the carbonized film in aviation washing gasoline, and then remove it by hand grinding or power tool polishing. However, this method has many disadvantages. First, the removal of the carbonized film is difficult and requires a lot of manpower and time. Secondly, the removal cycle is long, which seriously affects production efficiency and project progress. Most importantly, this method often cannot completely remove the carbonized film, and the residue may still interfere with fluorescent inspection. Summary of the invention
[0005] In view of the problems existing in the prior art, the present invention provides a method for removing the carbonized film of the laser-punched protective tape of an aviation blade, which can quickly and thoroughly remove the carbonized film while ensuring the integrity and performance of the blade, thereby improving the production efficiency and quality of the aviation engine.
[0006] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:
[0007] A method for removing a carbonized adhesive film of a laser-punched protective tape for an aviation blade, comprising:
[0008] Soak the pre-treated aviation blades in the remover for a set period of time and then take them out;
[0009] Post-process the soaked aviation blades.
[0010] Furthermore, the set duration is 1 hour to 3 hours.
[0011] Furthermore, when the pre-treated aviation blade is immersed in a remover, the method further comprises:
[0012] Ultrasonic waves or mechanical agitation are applied to the remover.
[0013] Furthermore, when the pre-treated aviation blade is immersed in a remover, the method further comprises:
[0014] The remover is heated to 60°C to 90°C.
[0015] Furthermore, before immersing the pre-treated aviation blade in the remover, the method further comprises:
[0016] The surface of the aviation blade is cleaned and dried using acetone or non-halogenated organic solvent cleaning agent.
[0017] Further, drying in air uses compressed air to dry the inner and outer surfaces of the aviation blades.
[0018] Furthermore, the post-processing of the immersed aviation blades includes:
[0019] Drain the soaked aviation blades from the residual remover.
[0020] Furthermore, after draining the residual remover from the soaked aviation blade, the method further comprises:
[0021] The drained aviation blades are washed with water.
[0022] Furthermore, after the drained aviation blades are washed with water, the method further comprises:
[0023] The cleaned aviation blades are dried.
[0024] Furthermore, the cleaning of the aviation blades is dried, specifically:
[0025] The aviation blades are placed in an oven at 60℃ to 80℃ for drying.
[0026] Compared with the prior art, the present invention has at least the following beneficial effects:
[0027] The present invention provides a method for removing the carbonized film of the protective tape on the laser drilling of aviation blades. Compared with the existing mechanical removal method of manual grinding or electric tool polishing after soaking in aviation washing gasoline, the removal method can not only reduce the labor intensity of personnel and avoid damage to the blade substrate caused by improper mechanical removal, but also can remove the carbonized film in multiple pieces at a time, quickly and efficiently, ensuring that the blade substrate is not damaged after laser drilling and the defect fluorescence inspection work can be carried out smoothly. In other words, the present invention can quickly and efficiently remove the carbonized film of the protective tape on the blade surface without damaging the blade substrate, avoiding the problem of blade damage caused by improper and incomplete mechanical removal and incomplete removal of the carbonized film, and providing a clean and complete substrate surface for fluorescence inspection of the blade processing surface.
[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are given below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] In order to more clearly illustrate the technical solutions in the specific implementation modes of the present invention, the drawings required for use in the description of the specific implementation modes will be briefly introduced below. Obviously, the drawings described below are some implementation modes of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0030] Figure 1 This is a flow chart of a method for removing a carbonized adhesive film of a protective tape for laser drilling of an aviation blade according to an embodiment of the present invention;
[0031] Figure 2 A schematic diagram of an auxiliary device used in a method for removing a carbonized adhesive film of a protective tape for laser drilling of an aircraft blade according to an embodiment of the present invention;
[0032] Figure 3 This is a metallographic diagram of an IC10 nickel-based high-temperature alloy sample after metallographic testing after immersion for 2 hours in an embodiment of the present invention.
[0033] In the figure: 1-accommodating slot; 2-hanging bracket; 3-hanging hook. DETAILED DESCRIPTION
[0034] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0035] The present application embodiment provides a method for removing the carbonized film of protective tape on laser-drilled aircraft blades, which aims to safely and efficiently remove the carbonized film of protective tape produced by laser drilling on high-pressure turbine blades. The specific implementation steps of this embodiment will be described in detail below:
[0036] Step 1: Pre-treatment
[0037] First, the surface of the aviation blade is pre-treated. Acetone or non-halogenated organic solvent cleaning agent is used to clean the pollutants on the blade surface after processing to ensure that the blade surface is clean and avoid pollutants such as oil stains that affect the effect of the remover.
[0038] After cleaning, dry the blades in the air, especially use compressed air to blow dry the inner and outer surfaces of the blades, especially the blind holes and grooves, to ensure that there is no water residue on the blade surface.
[0039] Step 2: Carbonized film removal
[0040] like Figure 2 As shown, the remover is loaded into a polyethylene or stainless steel containing tank 1 with a grid. Then, the cleaned and dried blades are hung by a hanging hook 3 provided on a hanging bracket 2 to ensure that the blades are completely immersed in the remover. The soaking time is set to 1 hour to 3 hours. Preferably, ultrasound or mechanical stirring can be applied during the soaking process as needed to accelerate the removal efficiency of the carbonized film.
[0041] More preferably, it has been verified that, if conditions permit, heating the remover to 60° C. to 90° C. can further improve the removal efficiency.
[0042] Exemplarily, the remover uses an alkaline ionic compound, and its main technical indicators are shown in Table 1 below:
[0043] Table 1 Technical requirements for alkaline ionic compound (complex polymer) removers
[0044] Serial number Technical requirements Technical indicators 1 Appearance Transparent to blue 2 <![CDATA[Density, g / cm 3 > 0.958-0.988 3 Flash point, °C 35-40 4 Boiling point, °C ≥100
[0045] Step 3: Drain the residual remover
[0046] After soaking, remove the blade from the remover and hang it over the remover tank to allow the residual remover on the blade to drain naturally. During this process, ensure that the residual remover in the blind holes and grooves of the blade is completely removed.
[0047] Step 4: Parts cleaning
[0048] After draining, rinse the leaves in clean, cold water to remove any remaining remover.
[0049] Preferably, in order to further ensure that the remover is completely removed, an air / water gun or high-pressure water may be used to wash the inner and outer surfaces of the blade, especially the blind holes and grooves.
[0050] Step 5: Drying the parts
[0051] After cleaning, use clean compressed air to blow dry the blades. Then, put the blades into an oven set at 60℃ to 80℃ for drying to ensure that the blades are completely dry for subsequent use.
[0052] Through the above steps, this method can safely and efficiently remove the carbonized film of the protective tape produced by laser drilling on the aviation blades without damaging the blade substrate. Compared with the existing mechanical method of manual grinding or electric tool polishing after soaking in aviation washing gasoline, this method not only reduces the labor intensity of personnel and avoids the damage to the blade substrate caused by improper mechanical removal, but also can achieve multiple pieces at a time, fast and efficient removal of the carbonized film, ensuring that the blade substrate is not damaged after laser drilling and the defect fluorescence inspection work can be carried out smoothly.
[0053] In one embodiment, the method of the present invention is tested as follows:
[0054] (1) Quality change test
[0055] The mass change test was conducted on IC10 nickel-based superalloy samples with a size of 10mm×10mm×4mm. Since the residual film was removed after immersion for 2 hours, a 5-fold removal time was selected for the mass change test. After the test, the unit mass change of the IC10 nickel-based superalloy sample met the requirement of <0.10g / cm 3 The specific requirements are shown in Table 2.
[0056] Table 2 IC10 sample mass change data before and after immersion
[0057]
[0058] (2) Metallographic structure test
[0059] Metallographic examination was carried out on IC10 nickel-based superalloy samples after immersion for 2 hours. Figure 3 As shown, no corrosion phenomenon was observed in the IC10 sample structure.
[0060] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "bottom", "inside", "outside", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0061] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.
[0062] In the present invention, unless otherwise clearly specified and limited, the terms "connected", "connection" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0063] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0064] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0065] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.
Claims
1. A method for removing the carbonized film of the protective tape for laser drilling of aircraft blades, characterized in that: include: Soak the pre-treated aviation blades in the remover for a set period of time and then take them out; Post-process the soaked aviation blades.
2. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 1 is characterized in that: The set duration is 1 hour to 3 hours.
3. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 1 is characterized in that: When the pre-treated aviation blade is immersed in the remover, the method further comprises: Ultrasonic waves or mechanical agitation are applied to the remover.
4. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 1 is characterized in that: When the pre-treated aviation blade is immersed in the remover, the method further comprises: The remover is heated to 60°C to 90°C.
5. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 1 is characterized in that: Before immersing the pre-treated aviation blade in the remover, the method further comprises: The surface of the aviation blade is cleaned and dried using acetone or non-halogenated organic solvent cleaning agent.
6. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 5 is characterized in that: Dry in air, using compressed air to dry the inner and outer surfaces of aviation blades.
7. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 1 is characterized in that: The post-processing of the immersed aviation blades comprises: Drain the soaked aviation blades from the residual remover.
8. The method for removing the carbonized film of the protective tape for laser drilling of aircraft blades according to claim 7 is characterized in that: After the soaked aviation blades are drained of the residual remover, the method comprises: The drained aviation blades are washed with water.
9. The method for removing the carbonized film of the laser-punched protective tape of an aircraft blade according to claim 8, characterized in that: After the drained aviation blades are washed with water, the method comprises: The cleaned aviation blades are dried.
10. The method for removing the carbonized film of the laser-punched protective tape of an aircraft blade according to claim 9, characterized in that: The drying process of the cleaned aviation blades is specifically as follows: The aviation blades are placed in an oven at 60℃ to 80℃ for drying.
Citation Information
Patent Citations
Method for ultrasonic removal of carbon deposition
CN103757650A
Method for cleaning up remains of aerospace craft pipeline
CN104438241A
Cleaning method of residual flow choking agent on surface of part
CN111744855A
Cleaning solution and cleaning method for coke on inner surface of renewable pipeline
CN112626528A
Method for removing residual glue and foreign matters of products in semiconductor packaging
CN115007539A