Method for preventing cold-rolled edge cracking by controlling hot rolling process of medium carbon steel
By controlling the hot rolling process of medium carbon steel, using soaking furnace heating, seven-stand hot rolling, laminar cooling and slow cooling processes, combined with angle steel shielding cooling, the problem of edge cracking in cold rolling of medium carbon steel was solved and the steel strip was improved. The performance uniformity and cold rolling efficiency reduce production costs.
Patent Information
- Application Number
- CN202410752262.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-15
AI Technical Summary
Medium carbon steel is prone to edge cracking defects during the cold rolling process, which affects cold rolling efficiency and increases costs.
It adopts the hot rolling process of soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes, and uses angle steel to shield the edge cooling of the hot-rolled steel strip to reduce the hardness and strength of the edge of the medium-carbon steel hot-rolled steel strip. , prevent the formation of martensite structure and improve the performance uniformity and plasticity of the steel strip.
It can effectively prevent cold-rolled edge cracking of medium-carbon steel, increase cold-rolling reduction, reduce cold-rolling passes and annealing processes, reduce production costs, and improve cold-rolling production efficiency and product yield.
Smart Images

Figure CN118768376A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of metallurgy, and in particular relates to a method for preventing cold-rolled edge cracking by controlling the hot-rolling process of medium-carbon steel. Background Art
[0002] Medium carbon steel has high strength, wear resistance and toughness, and is mainly used to manufacture mechanical parts and tools that require high strength and hardness. After cold rolling, medium carbon steel can obtain finer grains, improve the cold rolling performance, strength, hardness, wear resistance, etc. of medium carbon steel, and also improve the surface quality and dimensional accuracy of medium carbon steel plates. Therefore, mechanical parts for fine blanking need cold rolling. At present, medium carbon steel wide hot-rolled base materials are generally cold-rolled in two ways: one is to directly cold-roll the wide medium carbon steel hot-rolled base materials after pickling by a wide cold rolling mill; the other is to cold-roll the pickled and stripped base materials with a cold rolling mill corresponding to the width specifications after the wide medium carbon steel hot-rolled base materials are stripped. The direct cold rolling of the wide medium carbon steel hot-rolled base materials after pickling has high production efficiency, fewer processing steps, less cold-rolled steel strip trimming, high cold rolling yield, and more economical cold rolling costs; the cold rolling efficiency of the wide medium carbon steel hot-rolled base materials after stripping is relatively low, the yield is low, and the cold rolling cost increases. Because medium carbon steel has a relatively high carbon content and the strength of the hot-rolled base material is relatively high, the work hardening is obvious during the cold rolling process. Especially when the medium carbon steel is cold rolled with a large amount of reduction, it is very easy to produce cracking defects at the edge of the medium carbon steel with good quality at the edge of the hot-rolled base material. In severe cases, the strip breakage accident occurs, which greatly affects the improvement of the cold rolling efficiency of the medium carbon steel and increases the cold rolling cost of the medium carbon steel.
[0003] For example, Chinese patent CN107201436A discloses a process for producing thin-gauge medium carbon steel. In the invention, the obtained hot-rolled plate is subjected to two warm rollings, and each warm rolling has three rolling passes. The medium carbon steel without annealing is directly cold rolled with a large reduction, and the cold rolling reduction rate exceeds 45%. Due to the work hardening of the medium carbon steel caused by continuous cold deformation, the strength and hardness of the medium carbon steel hardened coil are increased. The medium carbon steel with good edge quality always has the problem of edge cracking during the cold rolling process. Summary of the invention
[0004] The object of the present invention is to provide a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, so as to solve the problem of edge cracking of medium carbon steel in the cold rolling process in the background technology.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] A method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, the method comprising soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling steps;
[0007] In the soaking furnace heating process, the medium carbon steel ingot produced by the CSP thin slab continuous casting machine is put into the soaking furnace for heating, the inlet temperature of the medium carbon steel ingot is 800-1000°C, the heating temperature is 1150-1250°C, and the temperature difference between the head and the tail of the medium carbon steel ingot is 0-40°C;
[0008] In the seven-stand hot rolling process, high-temperature rolling is first performed, and then the cooling water of the F1, F2, and F3 stands is turned on, the cooling water between the F4 and F5 stands is turned off, and the cooling water between the F6 and F7 stands is turned on to obtain medium carbon steel after hot rolling.
[0009] In the laminar cooling process, the front-stage concentrated cooling mode is selected for the hot-rolled medium carbon steel, and angle steel is used to shield the edge of the hot-rolled medium carbon steel in the laminar cooling. The cooling water does not cool the edge of the hot-rolled medium carbon steel to obtain a medium carbon steel hot-rolled steel strip.
[0010] The medium carbon steel hot-rolled steel strip in the coiling process is coiled and unloaded to obtain a medium carbon steel hot-rolled steel coil.
[0011] The medium carbon steel hot rolled coils in the slow cooling process are transported, spray-printed, and packaged via a conveyor chain, and are hoisted to a steel coil slow cooling pit for stack cooling to obtain stack cooled medium carbon steel coils.
[0012] Furthermore, the medium carbon steel ingot includes one of S50C and 45MnCr.
[0013] Furthermore, the high temperature starting rolling temperature is 1120-1180°C, and the final rolling temperature is maintained at 840-920°C.
[0014] Furthermore, the cooling water volume of the F1, F2, and F3 racks is opened by 20% respectively. When the cooling water is opened by 100%, the water flow rate is 320m 3 / h.
[0015] Furthermore, the angle steel blocks the edge of the medium carbon steel after hot rolling by 30mm-50mm.
[0016] Furthermore, the side spray water volume of laminar cooling is 60-120m 3 / h, during the cooling process, the cooling rate is controlled at 50-150℃ / s to ensure that the temperature of medium carbon steel is 620-740℃.
[0017] Furthermore, the stack cooling time is ≥72h or the temperature out of the buffer pit is ≤100°C.
[0018] Furthermore, the medium carbon steel coil after stack cooling is pickled with a hydrochloric acid solution with a mass concentration of 60-180 g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 45-55% to obtain cold-rolled medium carbon steel.
[0019] Furthermore, the width of the cold rolled medium carbon steel is 1200-1300 mm.
[0020] Beneficial effects of the present invention:
[0021] The present invention provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, comprising a hot rolling process of soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling; through the hot rolling process and the use of angle steel to shield the edge cooling of the steel strip in the hot rolling process, the hardness and strength of the edge of the medium carbon steel hot-rolled steel strip are reduced, the high hardness structure such as martensite is prevented from appearing at the edge of the medium carbon steel hot-rolled steel strip, the performance uniformity of the medium carbon steel hot-rolled steel strip is improved, and the plasticity and toughness of the edge of the medium carbon steel hot-rolled steel strip are improved, so that the edge strength of the medium carbon steel strip that has not been annealed is controlled to increase uniformly during the cold rolling process, even if When the cold rolling reduction is 45%, the medium carbon steel strip with good edge quality without annealing treatment will not have edge cracking defects, which is beneficial to increase the cold rolling reduction of medium carbon steel, reduce the rolling passes and medium carbon steel annealing process of cold rolling the medium carbon steel hot-rolled strip of the same thickness to the cold-hardened steel strip of the same thickness (reduce the cold rolling passes and annealing process under the same reduction conditions), reduce the number of annealing processes in the cold rolling production of thin-gauge medium carbon steel, reduce the production cost of cold rolling of medium carbon steel, and improve the production efficiency of cold rolling of medium carbon steel; at the same time, the cracking defects of cold rolling edges are reduced, the first-class rate of cold-rolled medium carbon steel is improved, and the production cost of cold rolling of medium carbon steel is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] The present invention will be further described below in conjunction with the accompanying drawings.
[0023] Figure 1 This is the edge quality diagram of the cold-rolled medium carbon steel produced in Example 1 (driving side);
[0024] Figure 2 This is the edge quality diagram (overall) of the cold-rolled medium carbon steel produced in Example 1;
[0025] Figure 3 The edge crack defect (driving side) of the cold-rolled medium carbon steel produced in Comparative Example 1;
[0026] Figure 4 This is the edge crack defect (driving side extension crack) of the cold-rolled medium carbon steel produced in Comparative Example 1. DETAILED DESCRIPTION
[0027] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] Example 1
[0029] This embodiment provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, including soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes, and the process steps are as follows;
[0030] The composition and weight percentage of the S50C slab steel produced by the CSP thin slab continuous casting machine are: C: 0.5184%, Si: 0.2126%, Mn: 0.6724%, P: 0.0169%, S: 0.0022%, Al: 0.0184%, and the rest is Fe and impurities;
[0031] Heating process of soaking furnace: S50C ingot is heated in soaking furnace at 800℃. When soaking furnace is heating S50C ingot, the heating temperature is controlled at 1150℃, and the temperature difference between head and tail is 20℃.
[0032] Seven-stand hot rolling process: The seven-stand hot rolling mill first performs high-temperature hot rolling at a temperature of 1120°C, and then the cooling water between the F1, F2, and F3 stands is opened by 20%, 20%, and 20% respectively. When the cooling water is 100% open, the water flow is 320m 3 / h, the cooling water between the F4 and F5 stands is turned off, the cooling water between the F6 and F7 stands is turned on, the final rolling temperature is controlled at 840°C, and the hot-rolled S50C strip is obtained;
[0033] Laminar cooling process: After hot rolling, the S50C strip selects the front concentrated cooling mode, and uses angle steel to shield the edge of the hot rolled medium carbon steel in the laminar cooling. The edge range is 30mm, and the measured water spray volume of the laminar cooling is 60m 3 / h, control the cooling rate to 50℃ / s, obtain S50C hot-rolled steel strip, and ensure that the temperature of S50C hot-rolled steel strip is 620℃;
[0034] Coiling process: After the S50C hot-rolled steel strip is coiled on the coiler, it is unloaded and sent to the conveyor chain;
[0035] Slow cooling process: The S50C hot-rolled steel coil is printed and packaged on the conveyor chain and then transported to the steel coil slow cooling pit for stack cooling. It is ensured that the S50C hot-rolled steel coil is statically and evenly slow-cooled in the slow cooling pit for 72 hours. The temperature out of the slow cooling pit is 95°C, and the S50C coil after stack cooling is obtained.
[0036] Cold rolling process: The S50C coil after stack cooling is pickled with a hydrochloric acid solution with a mass concentration of 90g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 45% and a width of 1200mm to obtain cold-rolled medium carbon steel.
[0037] The cold-rolled medium carbon steel produced in this embodiment has good surface quality during cold rolling production. A large sample is taken for observation. There are no micro cracks on the edge of the cold-rolled medium carbon steel, and no cold-rolled edge crack defects are produced on both sides. Figure 1 and Figure 2 (Example 2-4 Cold-rolled medium carbon steel edge quality diagram and Figure 1 and Figure 2 Similar, so omitted)
[0038] Example 2
[0039] This embodiment provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, including soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes, and the process steps are as follows;
[0040] This embodiment provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, including soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes;
[0041] The composition and weight percentage of the S50C slab steel produced by the CSP thin slab continuous casting machine are: C: 0.5184%, Si: 0.2126%, Mn: 0.6724%, P: 0.0169%, S: 0.0022%, Al: 0.0184%, and the rest is Fe and impurities;
[0042] Heating process in soaking furnace: S50C ingot is heated in soaking furnace at 1000℃. When soaking furnace is heating S50C ingot, the heating temperature is controlled at 1250℃, and the temperature difference between head and tail is 40℃.
[0043] Seven-stand hot rolling process: The seven-stand hot rolling mill first performs high-temperature hot rolling at a temperature of 1180°C, and then the cooling water between the F1, F2, and F3 stands is opened by 20%, 20%, and 20% respectively. When the cooling water is 100% open, the water flow is 320m 3 / h, the cooling water between the F4 and F5 stands was turned off, and the cooling water between the F6 and F7 stands was turned on, and the final rolling temperature was controlled at 920°C to obtain the S50C strip after hot rolling;
[0044] Laminar cooling process: After hot rolling, the S50C strip selects the front concentrated cooling mode, and uses angle steel to shield the edge of the hot rolled medium carbon steel in the laminar cooling. The edge range is 50mm, and the measured water spray volume of the laminar cooling is 120m 3 / h, control the cooling rate to 150℃ / s, obtain S50C hot-rolled steel strip, and ensure that the temperature of S50C hot-rolled steel strip is 740℃;
[0045] Coiling process: After the S50C hot-rolled steel strip is coiled on the coiler, it is unloaded and sent to the conveyor chain;
[0046] Slow cooling process: The S50C hot-rolled steel coil is printed and packaged on the conveyor chain and then transported to the steel coil slow cooling pit for stack cooling. It is ensured that the S50C hot-rolled steel coil is statically and evenly slow-cooled in the slow cooling pit for 96 hours. The temperature out of the slow cooling pit is 85°C, and the S50C coil after stack cooling is obtained.
[0047] Cold rolling process: The S50C coil after stack cooling is pickled with a hydrochloric acid solution with a mass concentration of 180g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 50% and a width of 1300mm to obtain cold-rolled medium carbon steel.
[0048] The cold-rolled medium carbon steel produced in this embodiment has no tiny cracks on the edge, and no cold-rolled edge crack defects are produced on both sides.
[0049] Example 3
[0050] This embodiment provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, including soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes;
[0051] The composition and weight percentage of 45MnCr slab steel produced by CSP thin slab continuous casting machine are: C: 0.4580%, Si: 0.2194%, Mn: 0.8604%, P: 0.0155%, S: 0.0021%, Cr: 0.2598%, Al: 0.0271%, and the rest is Fe and impurities;
[0052] Heating process of soaking furnace: 45MnCr ingot is heated in soaking furnace at 800℃. When soaking furnace is heating 45MnCr ingot, the heating temperature is controlled at 1150℃, and the temperature difference between head and tail is 20℃.
[0053] Seven-stand hot rolling process: The seven-stand hot rolling mill first performs high-temperature hot rolling at a temperature of 1120°C, and then the cooling water between the F1, F2, and F3 stands is opened by 20%, 20%, and 20% respectively. When the cooling water is 100% open, the water flow is 320m 3 / h, the cooling water between the F4 and F5 stands is turned off, the cooling water between the F6 and F7 stands is turned on, the final rolling temperature is controlled at 840°C, and the hot-rolled 45MnCr strip is obtained;
[0054] Laminar cooling process: The front concentrated cooling mode is selected for the hot-rolled 45MnCr strip, and the edge of the hot-rolled 45MnCr strip in the laminar cooling is shielded by angle steel. The edge range is 30mm, and the measured water spray volume of the laminar cooling is 60m 3 / h, control the cooling rate to 50℃ / s, obtain 45MnCr hot-rolled steel strip, and ensure that the temperature of 45MnCr hot-rolled steel strip is 620℃;
[0055] Coiling process: After the 45MnCr hot-rolled steel strip is coiled on the coiler, it is unloaded and sent to the conveyor chain;
[0056] Slow cooling process: The 45MnCr hot-rolled steel coils are printed and packaged on the conveyor chain and then transported to the steel coil slow cooling pit for stack cooling. Ensure that the 45MnCr hot-rolled steel coils are evenly slow-cooled in the slow cooling pit for 72 hours. The temperature out of the slow cooling pit is 95°C, and the 45MnCr coils after stack cooling are obtained.
[0057] Cold rolling process: After the stack cooling, the 45MnCr coil is pickled with a hydrochloric acid solution with a mass concentration of 70g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 45% and a width of 1200mm to obtain cold-rolled medium carbon steel.
[0058] The cold-rolled medium carbon steel produced in this embodiment has no tiny cracks on the edge, and no cold-rolled edge crack defects are produced on both sides.
[0059] Example 4
[0060] This embodiment provides a method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, including soaking furnace heating, seven-stand hot rolling, laminar cooling, coiling and slow cooling processes;
[0061] The composition and weight percentage of 45MnCr slab steel produced by CSP thin slab continuous casting machine are: C: 0.4580%, Si: 0.2194%, Mn: 0.8604%, P: 0.0155%, S: 0.0021%, Cr: 0.2598%, Al: 0.0271%, and the rest is Fe and impurities;
[0062] Heating process of soaking furnace: 45MnCr ingot is heated in soaking furnace at 1000℃. When soaking furnace heats 45MnCr ingot, the heating temperature is controlled at 1250℃, and the temperature difference between head and tail is 40℃.
[0063] Seven-stand hot rolling process: The seven-stand hot rolling mill first performs high-temperature hot rolling at a temperature of 1180°C, and then the cooling water between the F1, F2, and F3 stands is opened by 20%, 20%, and 20% respectively. When the cooling water is 100% open, the water flow is 320m 3 / h, the cooling water between the F4 and F5 stands is turned off, the cooling water between the F6 and F7 stands is turned on, the final rolling temperature is controlled at 920°C, and the hot-rolled 45MnCr strip is obtained;
[0064] Laminar cooling process: The front concentrated cooling mode is selected for the hot-rolled 45MnCr strip, and the edge of the hot-rolled 45MnCr strip in the laminar cooling is shielded by angle steel. The edge range is 50mm, and the measured water spray volume of the laminar cooling is 120m 3 / h, control the cooling rate to 150℃ / s, obtain 45MnCr hot-rolled steel strip, and ensure that the temperature of 45MnCr hot-rolled steel strip is 740℃;
[0065] Coiling process: After the 45MnCr hot-rolled steel strip is coiled on the coiler, it is unloaded and sent to the conveyor chain;
[0066] Slow cooling process: The 45MnCr hot-rolled steel coils are printed and packaged on the conveyor chain and then transported to the steel coil slow cooling pit for stack cooling. It is ensured that the 45MnCr hot-rolled steel coils are statically and evenly slow-cooled in the slow cooling pit for 96 hours. The temperature out of the slow cooling pit is 85°C, and the 45MnCr coils after stack cooling are obtained.
[0067] Cold rolling process: After the stack cooling, the 45MnCr coil is pickled with a hydrochloric acid solution with a mass concentration of 140g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 45% and a width of 1300mm to obtain cold-rolled medium carbon steel.
[0068] The cold-rolled medium carbon steel produced in this embodiment has no tiny cracks on the edge, and no cold-rolled edge crack defects are produced on both sides.
[0069] Comparative Example 1
[0070] Based on Example 2, the phrase "and using angle steel to shield the edge of the hot-rolled S50C strip during laminar cooling, with an edge range of 50 mm" in Example 2 is replaced with "the hot-rolled S50C strip is laminar cooled", and the remaining raw materials and process are the same as in Example 2.
[0071] The surface quality of the cold-rolled medium carbon steel produced in this comparative example is poor during cold rolling production. A large sample is taken for observation and it is found that there are tiny cracks on the edge of the strip and cold-rolled edge cracks on both sides. Figure 3 and Figure 4 .
[0072] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0073] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel, It is characterized in that The method comprises the steps of heating in a soaking furnace, hot rolling with seven stands, laminar cooling, coiling and slow cooling; In the soaking furnace heating process, the medium carbon steel ingot is placed in the soaking furnace for heating, the inlet temperature of the medium carbon steel ingot is 800-1000°C, the heating temperature is 1150-1250°C, and the temperature difference between the head and the tail of the medium carbon steel ingot is 0-40°C; In the seven-stand hot rolling process, high-temperature rolling is first performed, and then the cooling water of the F1, F2, and F3 stands is turned on, the cooling water between the F4 and F5 stands is turned off, and the cooling water between the F6 and F7 stands is turned on, so as to obtain medium carbon steel after hot rolling; In the laminar cooling process, the hot-rolled medium carbon steel is subjected to front-end concentrated cooling mode, and angle steel is used to shield the edge of the hot-rolled medium carbon steel during laminar cooling to obtain a medium carbon steel hot-rolled steel strip; The medium carbon steel hot-rolled steel strip in the coiling process is coiled and unloaded to obtain a medium carbon steel hot-rolled steel coil; The medium carbon steel hot rolled coils in the slow cooling process are transported, spray-printed, and packaged via a conveyor chain, and are hoisted to a steel coil slow cooling pit for stack cooling to obtain stack cooled medium carbon steel coils.
2. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The medium carbon steel ingot includes one of S50C and 45MnCr.
3. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The high temperature rolling start temperature is 1120-1180°C, and the final rolling temperature is maintained at 840-920°C.
4. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The cooling water volume of the F1, F2, and F3 racks is opened by 20% respectively. When the cooling water is opened by 100%, the water flow rate is 320m 3 / h.
5. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The edge range of the angle steel covering the medium carbon steel after hot rolling is 30mm-50mm.
6. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The side spray water volume of the laminar cooling is 60-120m 3 / h, during the cooling process, the cooling rate is controlled at 50-150℃ / s to ensure that the temperature of medium carbon steel is 620-740℃.
7. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The stack cooling time is ≥72h or the outlet temperature of the buffer pit is ≤100°C.
8. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The medium carbon steel coil after stack cooling is pickled with a hydrochloric acid solution with a mass concentration of 60-180g / L and then cold rolled on a single-stand 18-roller reversible rolling mill with a cold rolling reduction of 45-55% to obtain cold-rolled medium carbon steel.
9. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The width of cold rolled medium carbon steel is 1200-1300mm.
10. The method for preventing cold-rolled edge cracking by controlling the hot rolling process of medium carbon steel according to claim 1, It is characterized in that The medium carbon steel ingot is produced by a CSP thin slab continuous casting machine.
Citation Information
Patent Citations
Rolling technology for high-carbon steel in thin slab casting and rolling
CN104438326A
SAE8660 hot-rolled sheet and production technology thereof
CN106756578A
Hot rolling process for reducing edge cracks of cold-rolled dual-phase steel of 1200 MPa or above
CN114653750A
Preparation method of ultrahigh-strength automobile steel
CN117488040A
Production process of punch level cold rolled steel plate based on CSP technology
CN1974821A