Economical high-boron steel pilgering process for nuclear power

By using a composite rolling method with a cladding structure and appropriate rolling processes, the problem of cracking in high boron steel during rolling was solved, enabling the production of high boron steel plates with high efficiency and low consumption.

CN118768385BActive Publication Date: 2026-11-10HEBEI DAHE MATERIAL TECH CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410928737.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2026-11-10
Estimated Expiration
2044-07-11

AI Technical Summary

Technical Problem

High-boron steel is prone to edge cracking during rolling, has poor thermoplasticity, resulting in low rolling efficiency and poor forming quality.

Method used

A composite rolling method using a cladding system is employed, employing A36 carbon structural steel cladding and an aluminum foil isolation layer. Combined with appropriate heating and rolling temperatures, the amount of rolling deformation is controlled, and straightening treatment is carried out to ensure the quality of the rolled material.

Benefits of technology

This effectively avoids cracking of high-boron steel plates during the rolling process, improves forming quality and preparation efficiency, and reduces heat loss and material consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118768385B_ABST
    Figure CN118768385B_ABST
Patent Text Reader

Abstract

The application discloses an economic high-boron steel canning rolling process for nuclear power, which comprises the following steps: (1) preparing a cuboid high-boron steel blank; (2) processing a canning for rolling according to the size of the blank, the canning is not blocked at both ends of the head and tail, the high-boron steel blank is loaded into the canning, and the blank and the canning are separated by a separation layer with a thickness of less than or equal to 1 mm; (3) hot rolling: the high-boron steel blank after the canning is heated in a resistance furnace, the heating temperature is between 1050-1250 DEG C, the heat preservation time is 1-3 h, the open rolling temperature is 950-1050 DEG C, the final rolling temperature is greater than 900 DEG C, and the total deformation amount of the controlled rolling is between 70-80%; (4) straightening the rolled plate by using a straightening machine, and the straightening temperature is greater than 900 DEG C; and (5) removing the canning, grinding and milling the surface of the high-boron steel, and thus the required high-boron steel plate is obtained. The process solves the problem of the cracking of the rolled plate in the rolling process of the high-boron steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of steel rolling technology, specifically relating to an economical high-boron steel cladding rolling process for nuclear power. Background Technology

[0002] High-boron steel is made by adding boron to the existing stainless steel composition. Stainless steel itself has a certain gamma-ray shielding effect, and the addition of boron further enhances its ability to absorb thermal neutrons and gamma rays. It also possesses high strength and good toughness, making boron-containing stainless steel suitable not only as a shielding material but also as a structural material. However, because high-boron steel contains a large amount of brittle compound phases, its thermoplasticity is reduced, making it prone to edge cracking during rolling. Summary of the Invention

[0003] The purpose of this invention is to provide an economical rolling process for high boron steel cladding for nuclear power plants. The high boron steel billet is loaded into a cladding material of A36 for rolling, which reduces temperature loss during the rolling process, ensures stable rolling, and improves the preparation efficiency and quality of high boron steel plates.

[0004] To achieve the above objectives, the technical solution of the present invention is as follows: An economical high-boron steel cladding rolling process for nuclear power plants includes the following steps: (1) Preparation of cuboid high-boron steel billet; (2) A rolling sleeve is processed according to the billet size. The sleeve has no sealing at both ends. The high boron steel billet is loaded into the sleeve. The billet and the sleeve are separated by an isolation layer with a thickness ≤1mm. (3) Hot rolling: The high boron steel billet after being wrapped is placed in an electric resistance furnace for heating at a temperature between 1050-1250℃ and held for 1-3 hours; the initial rolling temperature is 950-1050℃ and the final rolling temperature is >900℃; the total deformation during rolling is controlled between 70-80%. (4) The rolled plate is straightened using a straightening machine at a straightening temperature greater than 900℃; (5) Remove the cladding, grind and cut the surface of the high boron steel to obtain the required high boron steel plate.

[0005] Furthermore, the material of the sheath described in step (2) of this invention is A36 carbon structural steel. A36 carbon structural steel has a low carbon content, good ductility, excellent weldability, and is easy to process.

[0006] Furthermore, the sleeve described in step (2) of the present invention is welded from four A36 carbon steel plates, one above and one below and one on the side.

[0007] Furthermore, the insulating layer in step (2) of this invention is aluminum foil. Aluminum foil can fill the gap between the sheath and the rolled sheet. Aluminum foil is relatively soft and inexpensive.

[0008] Furthermore, the hot rolling process in step (3) of the present invention involves 6-10 rolling passes.

[0009] Furthermore, in step (3) of the present invention, the reduction per pass during the rolling process is controlled at 10% to 30%.

[0010] Further, the high-boron steel of the present invention has the following composition: B: 1.5-2.0%; C: 0.04-0.08%; Si: 0.4-0.8%; Mn: 1.00-2.00%; Cr: 15-19%; V: 0.015-0.028%; Ti: 0.02-0.06%; Ni: 9-12%; N≤0.08%; P≤0.015%; S≤0.003%, with the balance being Fe and unavoidable impurity elements.

[0011] This invention addresses the issue of poor thermoplasticity in high-boron steel, which makes it prone to cracking during rolling. It provides a method using a cladding and composite stacking rolling process to efficiently and conveniently produce high-boron steel sheets with crack-free surfaces and uniform microstructure. The invention's principle and beneficial technical effects are as follows: (1) The combination of the cladding and the high boron steel billet reduces the difficulty of heat preservation control, and the cladding structure increases the heat capacity and reduces heat loss during the rolling process, which is conducive to improving the forming quality of high boron steel plates. In addition, the cladding has a head and tail unsealed structure, which reduces the use of consumables.

[0012] (2) A36 carbon structural steel has good ductility and weldability, making it easy to weld between cladding plates. This can prevent high boron steel plates from being crushed by the cladding during rolling and post-rolling cooling. The aluminum foil protective layer used between billets and between billets and cladding is inexpensive.

[0013] (3) In this invention, after the high boron steel plate is wrapped and rolled, the rolled material is straightened to ensure that the high boron steel plate has a good plate shape after the wrapping is removed.

[0014] (4) The high boron steel described in this invention has a brittle phase. During the rolling process, a cladding device is used for heat preservation, and appropriate initial rolling temperature and final rolling temperature are used to solve the problem of plate cracking during the rolling process. It is highly practical and has significant effects. Attached Figure Description

[0015] Figure 1 The encapsulation structure described in this invention; Figure 1 The ABCD and EFGH surfaces are the top and bottom surfaces of the sheath, respectively, while the ABEF and CDGH surfaces are the sides of the sheath.

[0016] Figure 2 The microstructure of the high boron steel plate in Example 1 is shown. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1

[0018] The high-boron steel composition in this embodiment is: B: 1.5%; C: 0.04%, Si: 0.7%, Mn: 1.00%, Cr: 15%, V: 0.028%, Ti: 0.04%; Ni: 11%; N: 0.06%; P: 0.01%, S: 0.003%, with the balance being Fe and unavoidable impurity elements; its rolling process is as follows: (1) Preparation of cuboid high boron steel billet: Ingots were prepared by vacuum consumable melting, and high boron steel slabs were obtained by 1100℃ billet treatment. The high boron steel slabs were processed into cuboid billets by machining, with a width of 210mm, a length of 360mm and a thickness of 120mm.

[0019] (2) The rolling sleeve is processed according to the billet size. A36 carbon structural steel is selected to process the sleeve. The sleeve is welded from four plates: the top, bottom, and side plates. Figure 1 As shown, the inner dimensions of the sheath are 211mm wide × 361mm long × 121mm thick. When welding the sheath, the two plates on the bottom and sides of the sheath are welded first. The milled high boron steel billet is then placed into the sheath. The billet and the sheath are separated by a 0.5mm thick aluminum foil isolation layer. After the billet is completely placed, the top and sides of the sheath are sealed by tungsten inert gas welding to ensure the strength and integrity of the weld. The overall thickness of the sheath is 30mm.

[0020] (3) Hot rolling: The high boron steel billet after being wrapped is placed in an electric resistance furnace for heating at 1120℃ and held for 2 hours; it is rolled using a hot rolling mill with a roll width of 550mm, with an initial rolling temperature of 950℃, a total of 6 passes, and a reduction of 20-30% per pass, and a final rolling temperature of 910℃; the thickness of the high boron steel plate after rolling is 30mm.

[0021] (4) Straightening: Straighten immediately after rolling using a straightening machine at a temperature above 900℃.

[0022] (5) Remove the casing by machining, take out the high boron steel plate, and grind and mill the high boron steel plate to make the surface smooth.

[0023] The high-boron steel plate in this embodiment is of good quality and shows no cracking; its microstructure is as follows. Figure 2 As shown; by Figure 2 It can be seen that the microstructure of high boron steel is mainly composed of austenite and FeCrB brittle phase. Example 2

[0024] The high-boron steel composition in this embodiment is as follows: B: 1.8%; C: 0.08%; Si: 0.4%; Mn: 1.5%; Cr: 17%; V: 0.02%; Ti: 0.02%; Ni: 9%; N: 0.07%; P: 0.015%; S: 0.002%; with the balance being Fe and unavoidable impurity elements.

[0025] Preparation of rectangular high-boron steel billets: First, ingots are prepared using a 50kg vacuum melting furnace. The ingots are then milled for rolling and coated with an anti-rust paint. The billet width is 150mm, length is 240mm, and thickness is 145mm.

[0026] (2) The rolling sleeve is processed according to the billet size. A36 carbon structural steel is selected to process the sleeve. The sleeve is welded from four plates: top, bottom, and side. Figure 1 As shown, the internal cavity dimensions are 150.6mm wide × 240.6mm long × 145.6mm thick. During the welding of the sheath, the bottom and side plates of the sheath are first welded together. The milled high-boron steel billet is then inserted into the sheath, separated from the sheath by a 0.5mm thick aluminum foil separator. After the billet is fully inserted, the top and sides of the sheath are sealed using tungsten inert gas welding to ensure weld strength and integrity. The overall thickness of the sheath is 20mm.

[0027] (3) Hot rolling: The high boron steel billet after welding and sheathing is placed in an electric resistance furnace for heating at 1250℃ and held for 1 hour; it is rolled using a hot rolling mill with a roll width of 350mm, with an initial rolling temperature of 970℃, a total of 10 passes, and a reduction of 10-20% per pass, and a final rolling temperature of 920℃; the thickness of the high boron steel plate after rolling is 35mm. (4) Straightening: Straighten immediately after rolling using a straightening machine at a temperature above 900℃.

[0028] (5) Remove the casing by machining, take out the high boron steel plate, and grind and mill the high boron steel plate to make the surface smooth.

[0029] The high-boron steel sheet in this embodiment is in good condition and shows no cracking. Example 3

[0030] The high-boron steel of this invention has the following composition: B: 2.0%; C: 0.05%; Si: 0.6%; Mn: 1.3%; Cr: 16%; V: 0.015%; Ti: 0.04%; Ni: 10%; N: 0.08%; P: 0.01%; S: 0.003%, with the balance being Fe and unavoidable impurity elements.

[0031] Preparation of rectangular high-boron steel billets: First, ingots are prepared using a vacuum melting furnace. The ingots are then milled for rolling. The melted billet has a width of 350 mm, a length of 370 mm, and a thickness of 150 mm.

[0032] The rolling sheath is fabricated according to the billet dimensions: A36 carbon structural steel is selected for the sheath, which is welded from four plates (top, bottom, and sides). The inner cavity dimensions are 150.2mm wide × 240.2mm long × 145.2mm thick. After welding, the high-boron steel billet is inserted into the sheath, and the space between the billet and the sheath is filled with 0.6mm thick aluminum foil. The overall thickness of the sheath is 20mm. Hot rolling: The high boron steel billet with the welded sheath is placed in an electric resistance furnace and heated to 1200℃ for 3 hours; the initial rolling temperature is 1050℃, and it is rolled in 10 passes with a reduction of 10-20% per pass, and the final rolling temperature is 940℃; the thickness of the rolled high boron steel plate is 30mm.

[0033] (4) Straightening: Straighten immediately after rolling using a straightening machine at a temperature above 900℃.

[0034] (5) Machining and cutting to remove the cladding, take out the high boron steel plate, and complete the grinding and milling of the high boron steel plate to make the surface smooth.

[0035] The high-boron steel sheet in this embodiment is in good condition and shows no cracking. Example 4

[0036] The high-boron steel of this invention has the following composition: B: 1.9%; C: 0.06%; Si: 0.8%; Mn: 1.8%; Cr: 19%; V: 0.02%; Ti: 0.06%; Ni: 12%; N: 0.04%; P: 0.013%; S: 0.003%; with the balance being Fe and unavoidable impurity elements.

[0037] Preparation of rectangular high-boron steel billets: First, ingots are prepared using a vacuum melting furnace, followed by electroslag treatment to improve steel purity. The electroslag-treated ingots are then machined and milled. The resulting billet has a width of 300 mm, a length of 410 mm, and a thickness of 160 mm.

[0038] The rolling sheath is fabricated according to the billet size: A36 carbon structural steel is selected for fabricating the sheath, which is welded from four plates: top, bottom, and sides. Figure 1 As shown, the inner cavity dimensions are 300.8mm wide × 410.8mm long × 160.8mm thick; after the sleeve welding is completed, the high boron steel billet is inserted into the sleeve, and the space between the billet and the sleeve is filled with 0.8mm thick aluminum foil, and the overall thickness of the sleeve is 25mm. Hot rolling: The high boron steel billet with the welded sheath is placed in an electric resistance furnace and heated to 1050℃ for 2 hours; the initial rolling temperature is 1020℃, and it is rolled in 7 passes with a reduction of 10-20% per pass, and the final rolling temperature is 920℃; the thickness of the high boron steel plate after rolling is 55mm. (4) Straightening: Straighten immediately after rolling using a straightening machine at a temperature above 900℃.

[0039] (5) Remove the casing by machining, take out the high boron steel plate, and grind and mill the high boron steel plate to make the surface smooth.

[0040] The high-boron steel sheet in this embodiment is in good condition and shows no cracking.

Claims

1. An economical high-boron steel cladding rolling process for nuclear power plants, characterized in that, Includes the following steps: (1) Preparation of cuboid high-boron steel billet; (2) A rolling sleeve is processed according to the billet size. The sleeve has no sealing at both ends. The high boron steel billet is loaded into the sleeve. The billet and the sleeve are separated by an isolation layer with a thickness ≤1mm. The sleeve is made of A36 carbon structural steel and the isolation layer is made of aluminum foil. (3) Hot rolling: The high boron steel billet after being wrapped is placed in an electric resistance furnace for heating at a temperature between 1050-1250℃ and held for 1-3 hours; the initial rolling temperature is 950-1050℃ and the final rolling temperature is >900℃; the total deformation during rolling is controlled between 70-80%. (4) The rolled plate is straightened using a straightening machine at a straightening temperature greater than 900℃; (5) Remove the cladding, grind and cut the surface of the high boron steel to obtain the required high boron steel plate.

2. The economical high-boron steel cladding rolling process for nuclear power plants according to claim 1, characterized in that, The sleeve in step (2) is welded from four A36 carbon steel plates, one on the top, one on the bottom, and one on the side.

3. The economical high-boron steel cladding rolling process for nuclear power plants according to claim 1, characterized in that, The hot rolling process in step (3) involves 6-10 passes.

4. The economical high-boron steel cladding rolling process for nuclear power plants according to claim 1, characterized in that, In step (3), the reduction per pass during the rolling process is controlled at 10% to 30%.

5. The economical high-boron steel cladding rolling process for nuclear power plants according to claim 1, characterized in that, The high-boron steel composition is: B: 1.5-2.0%; C: 0.04-0.08%, Si: 0.4-0.8%, Mn: 1.00-2.00%, Cr: 15-19%, V: 0.015-0.028%, Ti: 0.02-0.06%, Ni: 9-12%, N≤0.08%, P≤0.015%, S≤0.003%, with the balance being Fe and unavoidable impurity elements.

Citation Information

Patent Citations

  • Method for improving hot-working performance and room-temperature plasticity of high-boron stainless steel

    CN106702287A

  • 370MPa-grade stainless steel composite plate and preparation method thereof

    CN116001380A